| HS Code | 490340 |
| Density G Cm3 | 1.30 |
| Melt Volume Flow Rate Cm3 Per 10min | 20 |
| Melting Temperature C | 225 |
| Heat Deflection Temperature 0 45 Mpa C | 150 |
| Heat Deflection Temperature 1 8 Mpa C | 60 |
| Vicat Softening Temperature B C | 170 |
| Tensile Modulus Mpa | 2600 |
| Tensile Stress At Break Mpa | 55 |
| Tensile Strain At Break Percent | 15 |
| Charpy Notched Impact Strength 23 C Kj M2 | 3.0 |
| Molding Shrinkage Percent | 1.8 |
| Water Absorption Saturation Percent | 0.4 |
| Volume Resistivity Ohm Cm | 1E14 |
| Dielectric Constant 1 Mhz | 3.2 |
| Comparative Tracking Index V | 600 |
As an accredited Celanese Crastin® Unreinforced PBT S600F20 NC010 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Celanese Crastin PBT S600F20 NC010 is supplied in 25 kg moisture-barrier bags, 40 bags (1,000 kg) per pallet. |
| Container Loading (20′ FCL) | Celanese Crastin® Unreinforced PBT S600F20 NC010 is palletized, unitized, and securely loaded into a 20-foot FCL container for transport. |
| Shipping | Shipping description: Celanese Crastin® Unreinforced PBT S600F20 NC010, polybutylene terephthalate (PBT) resin pellets, natural. Non-hazardous, not DOT/IMDG/IATA regulated. Ship in dry, sealed packaging; protect from moisture, contamination, and excessive heat. Store in a cool, dry area. Use appropriate labeled containers and maintain lot identification. Avoid prolonged exposure to direct sunlight. |
| Storage | Store Celanese Crastin® Unreinforced PBT S600F20 NC010 in a cool, dry, well-ventilated area, away from direct sunlight, heat sources, oxidizing agents, and incompatible chemicals. Keep containers tightly closed in the original packaging to prevent moisture absorption and contamination. Avoid prolonged humid exposure; use desiccants if required and follow the supplier’s SDS and local regulations. |
| Shelf Life | Shelf life is typically 24 months from date of delivery when stored dry, cool, and in original unopened packaging under recommended conditions. |
Competitive Celanese Crastin® Unreinforced PBT S600F20 NC010 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Celanese Crastin® Unreinforced PBT S600F20 NC010 is an unpigmented natural polybutylene terephthalate injection-molding grade classified under ISO 1043 as PBT. The grade identifier combines the unreinforced S600 polyester series, the F20 medium-flow designation, and the NC010 natural-color code. Under ISO 1133-1:2022, melt volume-flow rate at 250 °C and 2.16 kg is positioned in the region of 20 cm³/10 min; this places the product between lower-flow extrusion-oriented PBT grades and higher-flow thin-wall grades. The absence of glass fiber or mineral reinforcement is the controlling variable in property differentiation: tensile modulus, creep resistance, and heat deflection temperature are lower than those of reinforced Crastin grades, while elongation, surface smoothness, and tribological behavior against polymer counterfaces are more favorable for unlubricated small mechanisms. The intended application envelope includes electromechanical housings, sensor bodies, relay bases, connector bodies, switch housings, and appliance control parts subjected to moderate mechanical load and short injection cycles. The material is not a drop-in replacement for glass-filled PBT in structural brackets or motor supports.
Material classification does not by itself establish food-contact or medical clearance. For food-contact use, the base PBT may be assessed under 21 CFR 177.1660 and EU Regulation 10/2011, but the final article requires migration testing under actual time-temperature conditions. Electrical and electronic parts should be evaluated against RoHS Directive 2011/65/EU Annex II restrictions for lead, mercury, cadmium, hexavalent chromium, and brominated flame retardants; the natural NC010 variant contains no carbon black or heavy-metal colorant, which supports formulations that must meet such restrictions, but incoming inspection and supplier documentation remain necessary. REACH compliance is article-dependent and should be confirmed through supplier declaration; the polymer itself is exempt from registration as a polymer under Title II, but monomers and substances of very high concern must be reviewed in the final compounded formulation.
PBT ester linkages degrade rapidly in the presence of moisture at processing temperature. The moisture limit for this grade is generally stated as 0.02% by weight; hydrolytic chain scission above this level lowers molecular weight, reduces melt strength, causes surface splay, and shifts the melt flow rate upward from the nominal 20 cm³/10 min region. Virgin pellets should be dried in a desiccant dryer at 120 °C for 4 h with a supply dew point of -40 °C or lower. Drying time must be extended when the pellet temperature at the dryer inlet is below 15 °C or when ambient relative humidity exceeds 60%. Regrind content above 25% should be avoided unless the drying hopper volume, residence time, and melt flow are verified every 2 h during production. At the press, hopper blanketing with dry air or nitrogen is recommended for open feed throats.
Melt temperature at the nozzle should normally remain between 240 °C and 260 °C for unfilled PBT. Residence time above 10 min at these temperatures, or melt temperature excursions above 270 °C, can produce yellowing, odor, and viscosity loss. A general-purpose screw with an L/D ratio of 20:1 to 25:1 and a compression ratio near 2.5:1 is commonly used; high-compression screws above 3:1 can generate excessive shear heating in the unfilled melt. Back pressure is typically set between 50 bar and 150 bar, but the actual set-point should be validated by shot-to-shot melt temperature uniformity within ±2 °C. Screw recovery speed should be reduced if melt temperature at the nozzle exceeds the set-point by more than 5 °C after a recovery cycle.
Representative values below are obtained from dry-as-molded specimens prepared under ISO 294-4 and are not specification limits. Tensile data follow ISO 527-1/-2; for comparison, ASTM D638-14 Type I specimens may generate slightly different values because of specimen geometry and test speed. Published data for this specific configuration is limited to standard specimen conditions; end-use design values must be generated on production tooling.
| Property | Test method | Representative value |
|---|---|---|
| Density | ISO 1183-1 | 1.31 g/cm³ |
| Melt volume-flow rate, 250 °C / 2.16 kg | ISO 1133-1:2022 | 20 cm³/10 min |
| Tensile modulus | ISO 527-1/-2 | 2500 MPa |
| Tensile stress at yield | ISO 527-1/-2 | 55 MPa |
| Nominal strain at break | ISO 527-1/-2 | >30% |
| Charpy notched impact strength, 23 °C | ISO 179-1/1eA | 3.0 kJ/m² |
| Heat deflection temperature, 1.8 MPa | ISO 75-1/-2 | 50 °C |
| Heat deflection temperature, 0.45 MPa | ISO 75-1/-2 | 150 °C |
| Comparative tracking index | IEC 60112 | 600 V |
| Flammability classification | UL 94 | HB |
The data explain the application boundary: the unfilled PBT carries short-term tensile stress but should not be used for continuous load-bearing service above 50 °C under 1.8 MPa load because heat deflection and creep resistance are limited in comparison with reinforced PBT. The notched impact is also outside the impact-modified range; snap-fit designs should avoid sharp notches and should be radiused at all gate vestiges. For dry electrical applications, the comparative tracking index is useful, but moisture uptake of approximately 0.4% under ISO 62 conditioning can alter surface resistivity and dissipation factor; creepage distances should be evaluated on the final assembly, not on the resin alone.
PBT crystallizes rapidly. In S600F20 NC010, mold temperature has a direct influence on post-mold dimensions. At mold temperatures between 60 °C and 90 °C, shrinkage after 24 h is generally stable. If the tool operates below 40 °C, the part may leave the mold with lower initial crystallinity and then continue to shrink over the first hour, causing dimensional drift in a supply chain. For tolerance-critical parts, the measurement protocol should fix conditioning at 23 °C and 50% relative humidity for 24 h before inspection. Water absorption after 24 h immersion at 23 °C can also increase dimensions by a small but measurable amount in humid service; this is not a defect but must be included in tolerance stack-ups.
Tooling conversion from glass-reinforced PBT to unfilled S600F20 NC010 requires re-establishment of shrinkage targets, pack pressure, venting, and cavity-pressure transfer. Glass-filled PBT shrinks less than unfilled PBT; an unfilled cavity may require pack pressures between 600 bar and 1000 bar, depending on wall thickness and gate freeze time. If the original tool used a gate diameter optimized for filled material, the unfilled grade may still fill because of its higher melt flow, but the gate may not seal at the same time; a larger gate or longer hold time may be needed to avoid sink marks opposite ribs. The switch-over from injection velocity to holding pressure should occur at 95% to 98% of cavity volume, confirmed by cavity-pressure sensors rather than by screw position alone.
Venting adjustments are necessary because unfilled PBT generates a faster flow front than filled grades at the same melt temperature. Parting-line vent depths are commonly held below 0.015 mm to avoid flash, but insufficient venting can produce burn marks at the end of fill. For multi-cavity tools, cavity-to-cavity fill imbalance below 5% by mass and cooling-water supply-return delta T below 2 °C are more important than average melt temperature alone. Cooling water temperature may be set between 60 °C and 90 °C to encourage crystallization and dimensional stability; mold temperatures below 40 °C can freeze thin ribs below 0.6 mm before full packing and produce surface delamination or weld-line weakness.
Production evaluations on a 1,000 kN electric injection molding machine with a 25 mm general-purpose screw have shown that pellet moisture and switch-over position are the most frequent causes of short-shot and flash variation. Batch-to-batch melt viscosity changes are ordinarily within the flow specification, but residence time and hopper moisture can cause larger shifts than the intrinsic polymer variation. To maintain shot-to-shot uniformity, the cushion should be held between 2 mm and 5 mm, screw decompression should not exceed 3 mm, and the cycle should not be interrupted without purging the barrel at low screw speed.
Hot-runner conversion is permitted, but nozzle tips must not overheat the melt. Temperature zones should be profiled so that the manifold is no more than 10 °C above the melt set-point and the tip is no more than 20 °C above the melt set-point. Unfilled PBT can degrade in hot-runner dead spots, creating black specks; therefore, flow paths should be streamlined and shut-off valve gates should be serviced before a run. For cold-runner tools, the sprue diameter should be sufficient to avoid premature gate freeze, typically 2.5 mm to 4.0 mm for a main runner, with the smaller end reserved for sub-runners and gates.
Ultrasonic welding of unfilled PBT requires high amplitude and a designed energy director; because the polymer is crystalline, a sharp melt transition means weld cycles are short, and a delay in trigger pressure can cause brittle joints. Vibration welding may be preferable for large planar parts, but the lower modulus of unfilled PBT relative to glass-filled PBT requires a wider wall section to prevent buckling. Adhesive bonding on natural PBT surfaces is improved by surface activation; without plasma or corona treatment, adhesion to cyanoacrylate or structural acrylics may be inconsistent. Laser marking of natural NC010 yields low contrast unless filler or marking additives are present, so pad printing, hot stamping, or inkjet with adhesion promoter should be used for permanent identification.
For continuous electrical service, the comparative tracking index of 600 V does not guarantee performance in polluted or high-humidity environments. The unfilled PBT absorbs moisture from air, and surface leakage current can increase under condensation. Mated connectors should be designed with adequate creepage and clearance per IEC 62368-1 or IEC 60335-1, depending on the end product. The material may be used in reinforced insulation only if the final assembly passes dielectric strength at the required voltage; the raw material alone does not constitute insulation class certification. For unattended appliance applications, glow-wire ignition temperature and glow-wire flammability index should be tested on the final part at the minimum wall thickness, with the final flame rating dependent on color and thickness.
PBT is not suitable for prolonged contact with strong bases, hydrolyzing aqueous media above 60 °C, and certain amine-based compounds, which can catalyze ester cleavage and lead to surface embrittlement. Automotive fluids, lubricating greases, and cleaning agents should be evaluated under the highest service temperature. In power tool and appliance housings, incidental contact with oils and detergents is usually acceptable, but stress-cracking resistance must be validated on parts with internal stress from inserts, weld lines, or press-fits. For dry sliding applications, unfilled PBT generates lower counterface wear than glass-filled PBT but may require external lubrication above 0.2 MPa surface pressure and 0.5 m/s sliding speed. Published data for the specific grade under boundary lubrication is limited; tribological qualification should be carried out on prototype components, not test plaques alone.
Compared with a lower-flow PBT grade in the same unreinforced family, the F20 derivative has higher melt volume-flow rate, which reduces injection pressure for the same cavity but may increase flash risk in worn tools or inadequately clamped molds. Compared with a representative 30% glass-filled PBT, the unfilled grade shows lower density, lower tensile modulus, lower heat deflection temperature, and higher mold shrinkage; the reinforced material is more appropriate for structural brackets and under-hood components with continuous thermal load. The unfilled material offers lower part mass, higher elongation, lower abrasive wear, and a smoother natural surface. These differences make S600F20 NC010 suitable for small precision housings and connectors, while reinforced PBT remains necessary where stiffness and dimensional stability at high load dominate.
Impact-modified unreinforced PBT grades contain elastomeric domains that raise notched impact, often above 10 kJ/m², but reduce tensile modulus and may lower chemical resistance. S600F20 NC010 lacks that elastomeric modification; it is not suitable for snap-fit parts that experience high-rate impact below 0 °C. In an enclosure with large snap latches, the wall and latch geometry should be re-evaluated or an impact-modified grade specified. Electrical or electronic components requiring V-0 classification under UL 94 cannot be satisfied by NC010 alone without flame-retardant modification, which would alter flow, moisture uptake, shrinkage, and mechanical behavior.