| HS Code | 156902 |
| Density | 1.31 g/cm³ |
| Water Absorption 24 H 23 C | 0.10% |
| Water Absorption Saturation | 0.40% |
| Tensile Modulus | 2,600 MPa |
| Tensile Stress At Break | 55 MPa |
| Nominal Strain At Break | 30% |
| Charpy Notched Impact Strength 23 C | 5 kJ/m² |
| Heat Deflection Temperature 0 45 Mpa | 150 °C |
| Heat Deflection Temperature 1 8 Mpa | 60 °C |
| Melting Temperature | 225 °C |
| Vicat Softening Temperature | 175 °C |
| Ul94 Flammability Rating | HB at 1.5 mm |
| Volume Resistivity | 1E15 ohm·cm |
| Dielectric Strength | 20 kV/mm |
| Comparative Tracking Index | 600 V |
| Molding Shrinkage | 1.5-2.0% |
As an accredited Celanese Crastin® Unreinforced PBT CE2055 NC010 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Celanese Crastin® Unreinforced PBT CE2055 NC010 is supplied in 25 kg bags, 40 bags per pallet (1,000 kg total). |
| Container Loading (20′ FCL) | 20′ FCL loads palletized 25 kg bags of Crastin CE2055 NC010 in a dry container; distribute evenly, secure, keep ambient, max ~20 t. |
| Shipping | Celanese Crastin® Unreinforced PBT CE2055 NC010 is a non-hazardous thermoplastic polyester resin supplied as pellets in moisture-barrier bags or boxes. Ship at ambient temperature, keep dry and away from heat, sunlight, and contamination. Not regulated as dangerous goods for transport; follow standard industrial hygiene and package handling precautions. |
| Storage | Store Celanese Crastin® Unreinforced PBT CE2055 NC010 in original, sealed packaging in a cool, dry, well-ventilated area, away from direct sunlight, heat, and moisture. Keep containers closed to prevent humidity pickup; dry before processing if needed. Use oldest stock first, keep away from incompatible chemicals, food, drink, and feed, and follow local regulations and manufacturer guidance. |
| Shelf Life | Typically 24 months from date of manufacture when stored unopened in original packaging, dry, below 30°C, and protected from sunlight. |
Competitive Celanese Crastin® Unreinforced PBT CE2055 NC010 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
The Celanese Crastin® CE2055 NC010 grade is an unreinforced polybutylene terephthalate injection-molding resin supplied in natural color. The NC010 designation identifies the natural, uncolored version, and the grade is not a PBT/PC alloy or a flame-retardant compound. Manufacturer-published typical values include a density of 1.31 g/cm³ according to ISO 1183 and a melt volume-flow rate of 31 cm³/10 min at 250 °C and 2.16 kg according to ISO 1133. The melt-flow position supports filling of thin-wall sections and multi-cavity tools, while the absence of glass fiber reduces tool wear and increases ductility relative to reinforced PBT. The grade should not be substituted into applications requiring a UL 94 V-0 listing or the stiffness of a glass-filled PBT without revalidating the part geometry and the certification file.
The most direct comparison is with 30 wt% glass-fiber-reinforced PBT. A typical glass-filled PBT grade exhibits a tensile modulus of 9000 MPa to 11000 MPa, while CE2055 NC010 is published at 2600 MPa under ISO 527-1/-2. The elongation at break moves in the opposite direction: CE2055 NC010 shows a nominal strain at break above 50%, whereas a glass-filled PBT may fracture below 5%. This property inversion creates a design boundary. Snap-fit arms, bosses, and living hinges originally computed for a filled PBT cannot be transferred to the unreinforced grade without increasing section thickness or redesigning the flexural element because the lower modulus reduces the force generated for the same deflection. Conversely, a part initially designed for unreinforced PBT may be over-stiffened by a glass-filled grade and may lose impact robustness due to reduced ductility. Within unfilled PBT grades, CE2055 NC010 is positioned for injection molding rather than extrusion. Extrusion-grade PBT typically has a lower melt volume-flow rate to maintain melt strength, whereas CE2055 NC010 reduces pressure drop in thin-wall sections but is less suitable for profile extrusion or blow molding where parison sag and draw-down resistance are required.
Compared with mineral-filled PBT, CE2055 NC010 has lower density, lower flexural modulus, higher elongation, and higher mold shrinkage. A mineral-filled PBT may be selected for warpage-sensitive parts because the mineral filler reduces shrinkage anisotropy, but it may also lower weld-line strength and surface gloss. Selection between the two materials should be based on ISO 294-4 shrinkage data and ISO 178 flexural modulus, not on material price per kilogram alone. Chemical and thermal differences also apply. Unfilled PBT of this type is semicrystalline and has a heat-deflection temperature under 1.8 MPa of approximately 50 °C. The unfilled grade should not be used for load-bearing components above this threshold unless stress levels are low and creep is accepted. PBT also hydrolyzes in hot water above 60 °C, which limits continuous service in aqueous environments and dictates drying practices in the molding plant.
In injection molding, the pellets are pre-dried before the feed throat because the condensation reaction in molten PBT is accelerated by moisture and thermal exposure. The supplier’s handling guidance for unfilled Crastin® PBT specifies drying in a desiccant-bed dryer at 120 °C for 4 h to 6 h when the material has been exposed to ambient air at relative humidity above 60%. A dew point of -40 °C or lower in the drying air is required to reach a final moisture content below 0.02 wt%. At moisture levels above this threshold, the melt hydrolyzes during processing, molecular weight drops, screw torque falls, and the notched impact strength of the molded part drops below the value obtained under ISO 179/1eA. The melt residence time at temperatures above 250 °C should not exceed 15 min; longer residence increases carboxyl end-group concentration and accelerates further hydrolysis. For standard injection molding machines with a general-purpose screw having an L/D ratio of 18:1 to 22:1 and a compression ratio of 2.5:1 to 3.5:1, the barrel profile is typically set from 230 °C at the rear zone to 260 °C at the nozzle. Tool temperature is maintained at 60 °C to 80 °C. A mold temperature below 50 °C freezes a highly amorphous skin and causes post-mold crystallization shrinkage when the part is heated or aged. Fill speed is set to prevent premature freeze-off in thin sections, but the shear rate should remain below 50,000 s⁻¹ to avoid local overheating and yellowing. Holding pressure is typically applied at 40 MPa to 70 MPa specific pressure until gate freeze, verified by plotting part mass against holding time and locating the plateau. Shot-to-shot mass variation is held within ±0.5% on production lines to avoid cavity imbalance. Hot-runner systems require manifold temperatures within 5 °C of the nozzle set point and elimination of dead spots where stagnant melt can degrade and generate black specks.
Melt-pressure measurements at the nozzle and hydraulic pressure readings should be monitored during production startups. A drop in nozzle pressure at constant injection velocity often indicates hydrolysis or check-ring leakage, whereas increasing pressure drop across the hot runner suggests degraded material accumulated in a dead zone. For unfilled PBT, a spiral-flow test can be used on a production line with a 2 mm spiral mold as a lot-to-lot consistency check, but the spiral length is not a specification and must be correlated with the current lot certificate. At high shear rates relevant to injection molding, the unfilled PBT exhibits pseudoplastic behavior; the apparent viscosity decreases as shear rate increases. The melt volume-flow rate of 31 cm³/10 min is a low-shear value and should not be used alone to predict pressure drop in thin-wall cavities above 1 mm. Capillary rheometry or mold-filling simulation should be employed to determine the pressure drop at the actual shear rate and temperature. Published capillary viscosity data for this specific grade is limited; therefore production trials with spider or sequential valve gating are recommended when wall thickness falls below 0.8 mm.
Gate geometry for unfilled PBT is set by the wall thickness and the viscosity; edge gates with a land length of 0.5 mm to 1.0 mm and a depth of 50% to 75% of the wall thickness are common. Submarine gates and tunnel gates should have adequate draft and radius to prevent shear heating; high shear at the gate can generate yellow streaks. The gate freeze time is typically in the range of 1 s to 3 s for thin-wall sections, but it must be confirmed experimentally because it depends on gate diameter and cooling rate.
The typical values in the table below are from the manufacturer’s published product data and are not release limits. Batch certificates should be consulted for lot-specific results. Values are obtained on dry-as-molded specimens unless otherwise noted. Specimen preparation for mechanical testing follows ISO 294-1 and ISO 294-4; test specimens are molded under controlled conditions to minimize orientation variability. Values determined by ISO 527-1/-2 are not numerically interchangeable with ASTM D638 results. The difference arises from specimen thickness, gauge length, and strain rate. A 50 mm/min ISO test and a 5 mm/min ASTM test produce different yield stress and elongation; direct substitution of one dataset into the other is not technically valid.
| Property | Typical value | Test method |
|---|---|---|
| Density | 1.31 g/cm³ | ISO 1183 |
| Melt volume-flow rate | 31 cm³/10 min | ISO 1133 at 250 °C/2.16 kg |
| Tensile modulus | 2600 MPa | ISO 527-1/-2 |
| Tensile stress at yield | 55 MPa | ISO 527-1/-2 |
| Nominal strain at break | >50% | ISO 527-1/-2 |
| Flexural modulus | 2300 MPa | ISO 178 |
| Flexural strength | 80 MPa | ISO 178 |
| Charpy notched impact strength | 4.0 kJ/m² | ISO 179/1eA at 23 °C |
| Izod notched impact strength | 4.0 kJ/m² | ISO 180/1A at 23 °C |
| Heat deflection temperature | 115 °C | ISO 75-2/B at 0.45 MPa |
| Heat deflection temperature | 50 °C | ISO 75-2/A at 1.8 MPa |
| Vicat softening temperature | 175 °C | ISO 306/B50 |
| Dielectric strength | 30 kV/mm | IEC 60243-1 |
| Comparative tracking index | 600 V | IEC 60112 |
| UL flame classification | HB | UL 94 at 0.75 mm |
Because PBT is semicrystalline, mold shrinkage and dimensional stability are governed by crystallization rather than simple thermal expansion. Manufacturer data for CE2055 NC010 list mold shrinkage values of approximately 1.4% to 1.5% under ISO 294-4. The unfilled grade produces higher absolute shrinkage than a 30 wt% glass-filled PBT, where fiber orientation suppresses parallel shrinkage to below 0.5%, but the unfilled grade often exhibits lower warpage in complex geometries because it lacks fiber-orientation anisotropy. Dimensional control requires uniform mold temperature; a cavity-to-cavity temperature difference above 15 °C can generate differential crystallinity and out-of-tolerance warpage in thin-wall parts. Post-mold annealing at 120 °C for 2 h can stabilize dimensions but increases crystallinity and may lower notched impact strength slightly.
The melting peak of PBT is typically near 225 °C under ISO 11357-3, and crystallization on cooling occurs between 180 °C and 200 °C. Mold temperature control in this band determines the crystalline microstructure. A higher mold temperature improves crystallization and dimensional stability but increases cycle time. A lower mold temperature produces a more amorphous shell and may lower the effective density; subsequent exposure to heat in service can then produce additional shrinkage. Shrinkage fixtures and metrology should therefore be performed after the part has equilibrated at ambient temperature for at least 24 h, or after annealing if the application temperature exceeds 80 °C. Water absorption at saturation is approximately 0.4% under ISO 62, which is low but sufficient to require drying before processing. Moisture absorbed during storage does not plasticize PBT to the same extent as polyamide, but it degrades the melt.
Electrical control housings are evaluated by IEC 60243-1, IEC 60112, and UL 94. Dry-as-molded CE2055 NC010 is published with a dielectric strength of 30 kV/mm and a comparative tracking index of 600 V. A CTI of 600 V places the material in the high tracking resistance category under IEC 60112, but this property is sensitive to surface contamination. Silicone-based external mold release agents should not be used on parts intended for creepage clearance control under IEC 60664-1 because the residue can alter surface tracking behavior. The unfilled grade’s elongation at break above 50% reduces the risk of cracking around molded-in metal inserts, but its low flexural modulus must be offset with ribbing or wall-thickness increases. For live parts, the end-use UL 94 classification must be confirmed on the actual part because the natural NC010 rating may not transfer to colored or thin-wall configurations; only the UL yellow card for the specific grade and thickness governs the certified classification.
Electrical testing is performed on dry-as-molded specimens; at equilibrium with 50% RH and 23 °C, the material may show a small reduction in surface resistivity and dielectric strength because water has a higher dielectric constant and can act as a surface contaminant. For humidity-sensitive applications, cleaning and drying before conformal coating is required. Stress-crack testing according to ISO 22088-3 should be used for applications involving solvents or aggressive media because the molded-in stress distribution, not just the base resin resistance, determines actual part failure. Additives that generate acidic byproducts should not be blended into the grade without testing, and regrind use should be limited to 20 wt% for critical parts unless lot-specific data supports a higher fraction.
Regulatory status for CE2055 NC010 is established through the supplier’s REACH registration, RoHS declaration, and current safety data sheet. The natural grade is generally covered under the manufacturer’s RoHS compliance program according to EU 2011/65/EU for lead, mercury, cadmium, hexavalent chromium, polybrominated biphenyls, and polybrominated diphenyl ethers. For food-contact use, the processor must obtain written confirmation from the supplier because unpublished additive packages may not automatically meet FDA 21 CFR 177.1660. Published data for specific food-contact configurations is limited, and PBT can stress crack in fatty foods and alcohols; therefore the final part must be tested under the intended food simulant and temperature. The material is not formulated for outdoor weathering, and long-term UV exposure should be addressed by the addition of a UV stabilization package or by selection of a UV-stabilized Crastin grade if outdoor service is required.
| Regulatory or standard reference | Scope | Processor action |
|---|---|---|
| RoHS 2011/65/EU | Restricted substances in electrical and electronic equipment | Confirm current lot declaration |
| REACH 1907/2006 | Registration and authorization status in EU | Check supplier SDS and registration number |
| UL 94 | Flammability class at thickness specified on yellow card | Verify actual part thickness and color |
| IEC 60664-1 | Insulation coordination for electrical equipment | Confirm creepage and clearance after contamination |
| FDA 21 CFR 177.1660 | Food-contact use of PBT | Obtain supplier confirmation only |
When an existing tool designed for 30 wt% glass-filled PBT is transferred to CE2055 NC010, the holding-pressure strategy must change because the unfilled material has lower melt viscosity but higher volumetric shrinkage. Holding pressure and packing time must be re-optimized, not simply reduced. The lower viscosity can produce flash at the same clamp force if the tool is worn, but the higher shrinkage can increase sink and shrink voids if the gate freezes too early. Clamp force requirements should be recalculated from the projected area and the melt pressure at the gate, not copied from the filled PBT process. Cooling time may require adjustment because glass fiber increases through-plane thermal conductivity; removing it reduces heat transfer in thicker sections. Mold temperature should remain at 60 °C to 80 °C. The fill speed profile may need to be faster in thin sections to avoid premature freeze-off, but the shear rate limit remains below 50,000 s⁻¹. Weld-line strength retention is usually better in unfilled PBT than in glass-filled PBT because no fiber orientation discontinuity occurs at the weld line; however, the absolute load capacity of the weld line remains lower than in the filled grade because the base modulus is lower. Tool wear is reduced with unfilled material, so existing hardened tool steel is acceptable but not mandatory from an abrasion standpoint. Hot-runner tips and valve-gate pins may need smaller clearances because the lower viscosity melt can leak through clearances that were acceptable for glass-filled PBT, producing stringing or gate drool.
Ribs and bosses originally designed for filled PBT should be checked for buckling and deflection. The unfilled material lowers stiffness under the same load by approximately the ratio of the two flexural moduli. If the glass-filled design used a flexural modulus of 9000 MPa and CE2055 NC010 is 2300 MPa, deflection increases by approximately 3.9× under identical geometry and load; section thickness must be increased or the part must be redesigned. Shrinkage is higher with unfilled PBT, so core pins and inserts may require increased draft or revised ejector placement to prevent ejection marks or sticking. If the application requires flame retardance, a glass-filled PBT tool cannot simply be converted to CE2055 NC010 unless the end-use regulatory requirement accepts the unfilled HB rating. If structural load capacity must be maintained, the wall thickness or rib geometry must be modified; a direct 1:1 replacement without redesign is not supported by the modulus data cited under ISO 527-1/-2.