| HS Code | 868135 |
| Product Name | Celanese Crastin® PBT+GF30%-FR-Black SK695FR BK507 |
| Polymer Base | PBT |
| Reinforcement | 30% glass fiber |
| Flame Retardancy | Flame retardant |
| Color | Black |
| Density | 1.64 g/cm³ |
| Molding Shrinkage Parallel | 0.3% |
| Molding Shrinkage Normal | 0.9% |
| Tensile Modulus | 10000 MPa |
| Tensile Stress At Break | 120 MPa |
| Tensile Strain At Break | 2.0% |
| Charpy Notched Impact Strength | 8 kJ/m² |
| Hdt At 1 8 Mpa | 200 °C |
| Hdt At 0 45 Mpa | 220 °C |
| Melting Temperature | 225 °C |
| Ul94 Flammability Rating | V-0 |
| Comparative Tracking Index | 600 V |
| Water Absorption | 0.3% |
As an accredited Celanese Crastin® PBT+GF30%-FR-Black SK695FR BK507 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Supplied in 25 kg net PE-lined moisture-proof bags, 40 bags per pallet (1,000 kg net). |
| Container Loading (20′ FCL) | 20′ FCL loaded with 25 kg bags of Celanese Crastin® PBT+GF30%-FR-Black SK695FR BK507, palletized, shrink-wrapped, and secured for ocean transport. |
| Shipping | Celanese Crastin® PBT+GF30%-FR-Black SK695FR BK507 is shipped as non-hazardous thermoplastic pellets in sealed moisture-barrier bags or octabins. It is not regulated for transport (no UN number). Keep dry, away from heat, contamination, and direct sunlight; handle according to SDS and package labeling. |
| Storage | Store in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, and open flames. Keep in original sealed packaging, tightly closed and off the ground to prevent moisture pickup and contamination. Avoid contact with strong oxidizers and incompatible chemicals. Maintain ambient temperatures, protect from physical damage, and follow the manufacturer’s SDS and local regulations. |
| Shelf Life | Shelf life is 24 months from production when stored unopened in original packaging, dry, below 30°C, protected from moisture and sunlight. |
Competitive Celanese Crastin® PBT+GF30%-FR-Black SK695FR BK507 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Celanese Crastin® PBT+GF30%-FR-Black SK695FR BK507 is a reinforced polybutylene terephthalate injection-moulding compound containing 30% glass fibre by weight and a halogenated flame-retardant package. The SK695FR designation belongs to the Crastin FR portfolio, and the BK507 suffix identifies the black colour formulation. The grade is used where thin-wall electrical enclosures, connectors, and structural insulating parts require a UL 94 V-0 flammability rating at 0.8 mm nominal thickness combined with high stiffness and heat resistance. Supplier documentation lists a typical density of 1.66 g/cm³ under ISO 1183-1, a tensile modulus of approximately 10,500 MPa under ISO 527-1/-2, and a tensile strain at break of 2.0–2.5%. The low elongation indicates that load-bearing features should avoid sharp internal corners and should be radiused to limit notch sensitivity.
| Property | Standard | Unit | Typical value |
|---|---|---|---|
| Density | ISO 1183-1 | g/cm³ | 1.66 |
| Tensile modulus | ISO 527-1/-2 | MPa | 10,500 |
| Tensile stress at break | ISO 527-1/-2 | MPa | 115 |
| Tensile strain at break | ISO 527-1/-2 | % | 2.0 |
| Flexural modulus | ISO 178 | MPa | 10,000 |
| Flexural strength | ISO 178 | MPa | 180 |
| Charpy notched impact, 23 °C | ISO 179-1/1eA | kJ/m² | 7.5 |
| Charpy notched impact, -30 °C | ISO 179-1/1eA | kJ/m² | 6.5 |
| Melt volume-rate, 250 °C/2.16 kg | ISO 1133-1 | cm³/10 min | 8 |
| Melting temperature | ISO 11357-1/-3 | °C | 225 |
| Heat deflection temperature, 1.8 MPa | ISO 75-1/-2 | °C | 200 |
| Comparative tracking index | IEC 60112 | V | 250 |
| Mould shrinkage, parallel | ISO 294-4 | % | 0.2–0.4 |
| Mould shrinkage, transverse | ISO 294-4 | % | 0.8–1.0 |
| Flammability rating, 0.8 mm | UL 94 | class | V-0 |
Values are typical for injection-moulded plaques conditioned at 23 °C and 50% relative humidity according to ISO 291; they are not specification limits. Lot-to-lot variation in glass length and flame-retardant dispersion can shift notched impact by ±1 kJ/m². Electrical performance depends on wall thickness and conditioning. The comparative tracking index of 250 V under IEC 60112 places the grade in a category that is lower than some unfilled FR-PBT formulations; this must be considered when calculating creepage distances under IEC 60664-1. Surface resistivity and volume resistivity are typical of glass-filled PBT but decline under prolonged humidity exposure, so open terminal layouts above 125 V require an assessment of pollution degree and creepage path.
Pre-drying is a critical threshold. Because PBT undergoes hydrolytic chain scission during plastication, residual moisture must be reduced below 0.02% prior to melting. A closed-loop desiccant dryer supplied with air at a dew point below -30 °C and set at 120 °C for 4 hours is the standard preparation. At 80 °C, drying time extends to 8 hours; temperatures above 130 °C risk pellet discolouration and flame-retardant decomposition. At relative humidity above 60%, dried pellets should be processed within 30 minutes or maintained in a hopper dryer at 100 °C. If surface streaking or nozzle gas evolution is observed, moisture levels should be rechecked with a Karl Fischer titrator according to ISO 15512 before adjusting other parameters.
Barrel setpoints should be adjusted to produce a melt temperature between 250 °C and 270 °C measured by air-shot pyrometry. The nozzle heater is typically set 5 °C below the front zone to minimise drool without freezing the gate. Tool temperature should be held between 60 °C and 100 °C; higher mould temperatures improve surface finish and crystallinity but increase cycle time and gas deposit formation on polished surfaces. Back pressure in the range 0.3–0.7 MPa and peripheral screw speed of 0.1–0.3 m/s are recommended for homogeneous glass distribution and flame-retardant dispersion. Residence time at melt temperature should not exceed 5 minutes; longer residence darkens the compound and generates acidic decomposition species that accelerate corrosion of unprotected tooling.
General-purpose screws with 20:1 to 25:1 L/D and compression ratio 2.0:1 to 2.5:1 are preferred over high-compression barrier screws. Glass fibre length retention is highest when the screw has gradual compression and no high-shear mixing elements. Check-ring wear should be monitored every 6–8 weeks because glass-filled FR-PBT is abrasive; bimetallic barrels and hardened screw flights are required for continuous production. Tool wear is progressive rather than sudden. In high-volume connector moulding, gate inserts can show land wear after 100,000 shots, changing gate dimensions and part dimensions. Replaceable gate inserts and defined dimensional audit intervals are recommended.
Common moulding defects on production equipment include gate blush, glass-fibre streaking, burn marks at venting, and brown streaking from thermal degradation. Gate blush is observed when injection velocity exceeds 200 mm/s at melt temperature 260 °C in a 1.0 mm wall connector; reducing injection speed to 120–160 mm/s and increasing gate diameter to 0.8 mm eliminates jetting. Brown streaks and acrid odour indicate residence time beyond 5 minutes or hot spots in the hot runner; the manifold should be set at 255 °C and all dead spots eliminated. Burn marks at the flow front are usually caused by insufficient venting; vents of 0.01–0.02 mm depth on the parting line should be maintained. Halogen-acid generation during melt processing requires tool maintenance. Unprotected low-alloy steel surfaces may show pitting after 30,000–50,000 cycles; chrome plating or nitrided surfaces extend tool life. Silicone-based mould releases should be avoided because surface contamination can interfere with ultrasonic welding and printing adhesion.
Mould shrinkage parallel to flow is 0.2–0.4% and transverse shrinkage is 0.8–1.0% under ISO 294-4; this anisotropy creates bowing in flat mouldings when wall thickness varies. For a 100 mm long connector body, differential cooling can produce out-of-flatness greater than 0.5 mm; tool designs should avoid thick bosses near flow entrances and should place gates away from thin walls to balance fill. Dimensional capability is influenced by hold pressure and gate seal. A short shot at gate seal is unreliable; hold pressure should be raised until part weight plateaus, then set 10–15% above that threshold. Cavity pressure for thin-wall connector tools is typically 40–60 MPa; minimum clamp force may be estimated from projected area multiplied by this cavity pressure.
Reground sprues and runners can be used at levels up to 20% by weight without significant loss of mechanical properties, provided the regrind is dry. Beyond 20%, fibre attrition reduces notched impact and increases mould shrinkage variation. If dimensional capability is critical, virgin material is recommended for production runs requiring ±0.05 mm tolerances. Mould temperatures below 40 °C produce low crystallinity, lower heat-deflection temperature, and increased post-moulding shrinkage; the melting peak near 225 °C under ISO 11357-1/-3 imposes a minimum tool temperature of 60 °C for adequate crystallinity and dimensional stability.
SK695FR BK507 is not a direct replacement for non-flame-retardant 30% glass-filled PBT. The flame-retardant system increases density from roughly 1.53 g/cm³ to 1.66 g/cm³, reduces tensile stress at break by approximately 10–15%, and lowers the comparative tracking index. Melt processing is also more constrained: the upper melt temperature of 270 °C is lower than many non-FR PBT-GF30 grades, and the acidic decomposition products require corrosion-resistant tooling and local exhaust ventilation. Compared with halogen-free FR-PBT-GF30, SK695FR BK507 generally offers lower melt viscosity and thinner-wall flame retardance but lower comparative tracking index and acidic gas release during processing. Halogen-free phosphorus-nitrogen systems may require higher additive loadings, raising density and reducing flow, but they avoid halogen-acid corrosion and may satisfy OEM halogen-free requirements.
Compared with unfilled FR-PBT, the grade offers a higher continuous-use deflection temperature and lower creep under mechanical load, but lower notched impact and higher melt viscosity. The 30% glass reinforcement raises tensile modulus from approximately 3,000 MPa to 10,500 MPa and raises heat-deflection temperature at 1.8 MPa from approximately 80 °C to 200 °C, while melt volume-rate at 250 °C/2.16 kg falls from values above 20 cm³/10 min for unfilled grades to approximately 8 cm³/10 min. The lower melt volume-rate reduces filling in walls below 0.5 mm; for such applications, a higher-flow Crastin FR grade should be evaluated. The glass also changes failure mode from ductile yield to brittle fracture at stress concentrators, which has implications for threaded inserts, snap-fits, and ultrasonic welding joints.
Within the Crastin SK-series, the numerical suffix does not refer solely to glass content but to a specific viscosity and flame-retardant formulation. SK695FR BK507 is often selected where a balance of flow and stiffness is required; SK605FR and SK603FR variants may differ in UL minimum thickness, flow length, or impact response. Published data for this specific configuration is limited for side-by-side comparisons, so any substitution should be validated by moulding trials and UL file verification. Against impact-modified PBT-GF30 FR grades, SK695FR BK507 shows lower notched impact and higher stiffness; impact-modified variants should be selected if Charpy notched impact above 10 kJ/m² is required.
Electrical connector insulators, relay bases, coil bobbins, terminal blocks, circuit-breaker arc chambers, sensor housings, and power-tool trigger bodies are typical production parts. In these applications, the material is exposed to short-term soldering or infrared reflow temperatures up to 250 °C; the 200 °C heat-deflection temperature at 1.8 MPa provides dimensional stability during insertion and soldering, but sustained exposure above 140 °C in hot air can embrittle the PBT matrix. Lead-free wave soldering at 255 °C for 3–5 seconds is generally compatible if the part is supported; infrared reflow with peak temperatures above 260 °C can cause blistering if the material contains residual moisture. Ultrasonic welding should use low amplitude and high welding force because the glass-filled matrix transmits vibration poorly; shear joints are preferred over butt joints, and flame-retardant additives may reduce weld strength by 10–20% relative to non-FR PBT-GF30.
Flame-retardant performance is usually stated as UL 94 V-0 at 0.8 mm. For unattended appliance applications, glow wire ignition temperature under IEC 60695-2-13 and glow wire flammability index under IEC 60695-2-12 may be required; many glass-filled PBT FR grades achieve a glow wire flammability index of 960 °C at 1.0 mm, but this value is material-specific and should be confirmed from the UL Yellow Card. The halogenated flame-retardant package provides rapid self-extinguishing under electrical fault conditions but is not recommended for parts exposed to hot water, steam, strong alkalis, or concentrated acids because PBT hydrolyses and the flame-retardant system can leach. Ventilation should remove melt emissions during processing.
RoHS compliance under Directive 2011/65/EU and REACH should be confirmed through the supplier’s Safety Data Sheet and UL Yellow Card. The grade contains a halogenated flame-retardant system; it is not a halogen-free compound. If an original equipment manufacturer requires halogen-free insulation per IEC 61249-2-21 or equivalent, SK695FR BK507 is not the appropriate selection.