| HS Code | 339210 |
| Glass Fiber Content | 20% |
| Density | 1.45 g/cm³ |
| Molding Shrinkage Parallel | 0.4% |
| Molding Shrinkage Normal | 0.9% |
| Tensile Modulus | 7000 MPa |
| Tensile Stress At Break | 120 MPa |
| Tensile Strain At Break | 3.0% |
| Flexural Modulus | 6500 MPa |
| Charpy Notched Impact Strength 23 C | 6 kJ/m² |
| Heat Deflection Temperature 1 8 Mpa | 200°C |
| Melting Temperature | 225°C |
| Processing Melt Temperature | 240-270°C |
| Mold Temperature | 80-100°C |
| Water Absorption Saturation | 0.4% |
As an accredited Celanese Crastin® PBT+GF20% SK603 NC010 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Celanese Crastin® PBT+GF20% SK603 NC010 is supplied in sealed 25 kg moisture-barrier bags, palletized for industrial handling. |
| Container Loading (20′ FCL) | Celanese Crastin® PBT+GF20% SK603 NC010 is palletized in 25 kg bags and loaded into a 20′ FCL for dry, secure stowage. |
| Shipping | Celanese Crastin® PBT+GF20% SK603 NC010 is a glass-fiber-reinforced PBT resin supplied as natural-color pellets. It is typically not regulated as dangerous goods for transport; ship in dry, clean, closed packaging at ambient temperature, protected from moisture and contamination. Confirm classification against the current SDS and local regulations. |
| Storage | Store Celanese Crastin® PBT+GF20% SK603 NC010 in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, and open flames. Keep containers tightly closed to prevent moisture pickup and contamination. Protect from dust and static buildup. Use original packaging, follow local regulations, avoid prolonged storage above recommended temperatures, rotate stock, and inspect containers regularly. |
| Shelf Life | Typically 24 months from date of manufacture when stored unopened in a cool, dry environment per Celanese recommendations. |
Competitive Celanese Crastin® PBT+GF20% SK603 NC010 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Celanese Crastin® PBT+GF20% SK603 NC010 is a natural-colour, 20% by weight glass-fibre-reinforced polybutylene terephthalate injection-moulding compound. The ISO 1043-1 designation is PBT-GF20; the suffix NC010 identifies the natural, uncolored pellet form. The resin is intended for conventional reciprocating-screw injection moulding rather than film extrusion or blow moulding. The reinforcement level is positioned between unfilled PBT and 30% glass-reinforced PBT to increase modulus, strength, heat deflection temperature, and dimensional control while retaining better flow than higher-glass compounds. The grade carries a standard UL 94 HB flammability classification; it is not flame-retardant and is not supplied with a V-0 rating. Celanese nomenclature for this product family uses the Crastin® trade name, the chemical family PBT, the filler description GF20%, and the alphanumeric grade code SK603. Other suffixes denote color-matched or stabilised variants. The SK603 grade is not identical to a generic PBT-GF20 reprocessed compound; proprietary stabilisers and release agents affect melt viscosity, plate-out, and long-term thermal stability. Buyers specifying this product should reference the full trade name and the batch certificate rather than only the ISO 1043 designation. The following data are representative values from manufacturer technical literature and standardized specimen tests; formal production release limits must be taken from the batch certificate.
Table 1 lists representative data measured on injection-moulded specimens according to Celanese and ISO methods. The tensile modulus of approximately 6800 MPa, measured by ISO 527-1/-2, is roughly 2.6 times the modulus of unfilled PBT and reflects the load-transfer effect of glass fibres oriented in the flow direction. Because fibre orientation is anisotropic, properties measured on edge-gated plaques differ from values measured on centre-gated plaques; moulded-part design should account for weld-line strength reduction relative to bulk tensile strength. The notched Charpy impact energy by ISO 179-1/1eA is approximately 6.0 kJ/m²; this places the grade in the moderately tough PBT range, with lower crack-initiation energy than unfilled PBT but higher resistance than many mineral-filled grades. The heat deflection temperature under 1.80 MPa loading by ISO 75-1/-2 is approximately 190°C, indicating that short-term dimensional stability under load is significantly higher than the 55–60°C HDT of unfilled PBT. The melting temperature of 225°C by ISO 11357-1/-3 imposes an upper processing limit because polyester degradation accelerates above approximately 280°C in the presence of residual moisture.
| Property | Test method | Typical value |
|---|---|---|
| Density | ISO 1183-1 | 1.45 g/cm³ |
| Tensile modulus | ISO 527-1/-2 | 6800 MPa |
| Tensile stress at break | ISO 527-1/-2 | 100 MPa |
| Tensile strain at break | ISO 527-1/-2 | 3.0% |
| Flexural modulus | ISO 178 | 6000 MPa |
| Flexural strength | ISO 178 | 160 MPa |
| Charpy notched impact strength, 23°C | ISO 179-1/1eA | 6.0 kJ/m² |
| Charpy unnotched impact strength, 23°C | ISO 179-1/1eU | 40 kJ/m² |
| Melting temperature, 10°C/min | ISO 11357-1/-3 | 225°C |
| Heat deflection temperature, 1.80 MPa | ISO 75-1/-2 | 190°C |
| Heat deflection temperature, 0.45 MPa | ISO 75-1/-2 | 215°C |
| Mould shrinkage, parallel flow direction | ISO 294-4 | 0.3% |
| Mould shrinkage, normal flow direction | ISO 294-4 | 1.0% |
| Water absorption, saturation at 23°C | ISO 62 | 0.35% |
| Flame rating at 1.6 mm | UL 94 | HB |
Because glass fibres orient during filling, properties measured on ISO specimens do not transfer directly to the moulded part. Flow-direction tensile modulus can exceed cross-flow modulus by 20–30%, and weld lines generated downstream of holes or multiple gates typically retain 50–60% of the nominal tensile strength. Finite-element simulation using anisotropic material coefficients is therefore required for structural components. The notched Charpy energy of 6.0 kJ/m² represents crack-initiation resistance; crack propagation, especially along weld lines, is less tolerant. Under sustained load, creep resistance remains acceptable below 80°C, but exposure to hot water or glycol above this temperature can accelerate stress relaxation. Published high-cycle fatigue data for this specific configuration is limited; S-N qualification should be performed on moulded plaques with the same fibre orientation as the final part.
The hydrolytic sensitivity of PBT dictates closed-loop drying. Manufacturer guidance for glass-reinforced PBT calls for drying at 120°C for 4 h in a desiccant dryer with a dew point of -30°C or lower, or for 6 h in a circulating air oven, to achieve maximum residual moisture of 0.02% by weight. In production environments with relative humidity above 60%, hopper dryers are inadequate because regrind and virgin pellets reabsorb surface moisture. Melt temperature should be kept between 250°C and 270°C, with a barrel profile from approximately 230°C at the feed throat to 255°C at the nozzle. Residence time above the melt temperature should not exceed 10–12 min; longer residence reduces molecular weight and darkens the natural resin. The screw should have an L/D ratio of 18:1 to 24:1 and a compression ratio of 2:1 to 2.5:1; reverse-taper nozzles and positive shut-off are required. Mould temperature should be held at 60–100°C, with 80°C preferred for dimensional stability; mould temperatures below 40°C reduce crystallinity and lower the effective HDT. Back pressure of 0.3–0.7 MPa and screw speeds below 100 rpm limit glass-fibre attrition. Injection pressures on production equipment typically range from 80 MPa to 140 MPa hydraulic, with hold pressures 60–100% of injection peak. Hold time is determined by gate freeze, but should not exceed 8–12 s for small gates; overpacking increases density and moulded-in stress. For hot-runner multi-cavity tools, sequential valve-gate opening reduces fill imbalances produced by the anisotropic viscosity of glass-filled PBT.
Fibre-length reduction is the dominant cause of lot-to-lot mechanical variation. On a 20:1 L/D general-purpose screw with a worn check ring, mean fibre length after plastication may fall to 300–500 μm, compared with the original chopped-strand length of 3–4 mm. The use of regrind above 20% by weight can reduce impact toughness by 15–25% because repeated plastication shortens fibres. Hot-runner gates below 1.0 mm diameter can cause fibre plugging; valve-gate or open pin gates of at least 1.0 mm are preferred. On actual multi-cavity tools with shear-sensitive manifolds, moulders sometimes observe cavity-to-cavity tensile modulus differences of 5–10% due to fibre orientation variation; this is reduced by balancing runner geometry rather than increasing hold pressure alone.
Electrical connector carriers, relay sockets, sensor housings, and power-tool shells are typical applications for SK603 NC010. The grade’s low water absorption of 0.35% by ISO 62 gives better dimensional stability in humid environments than polyamide 66 glass-reinforced compounds, which can absorb several percent moisture. For high-pin-count connectors, flat injection profiles and mould temperatures near 80°C minimize warpage. The short-term heat resistance provided by a 190°C HDT at 1.80 MPa permits limited exposure to soldering heat and oven curing, but continuous use above 150°C is outside the intended range. Electrical insulation characteristics are typical for natural PBT GF20, with volume resistivity near 1×10¹⁵ Ω·cm under IEC 62631-3-1 and dielectric strength of approximately 20 kV/mm for a 1.6 mm plaque under IEC 60243-1; creepage and clearance design must follow IEC 60664-1 because moulded surface roughness can reduce tracking resistance. Comparative tracking index values must be verified on the final moulded part under IEC 60112, because the surface distribution of glass fibres influences tracking resistance.
Glass-fibre orientation is not random in the moulded part. The skin layer consists of highly oriented fibres in the flow direction, while the core may be more cross-oriented; this produces a layered modulus profile. Under bending loads, the surface layers dominate, so flow-direction flexural modulus of ISO 178 specimens is higher than cross-flow values. At a weld line, fibres remain parallel to the interface instead of bridging it, and the result is a local tensile-strength reduction of up to 40–50% compared with the parent material. Ribs, bosses, and snap-fit arms located on a weld line can fail at nominal strains far below the 3.0% tensile strain at break measured on ISO 527-1/-2 specimens. Designers should place gates so that weld lines fall in low-stress regions, or use flow leaders to move the weld line. For snap-fit features, the maximum outer-fibre strain should be kept below 1.0%; higher strain can initiate cracking at exposed fibre ends. The thermal expansion coefficient is anisotropic, and published values for this exact grade are limited; measurements on plaques are recommended for tight-tolerance assemblies.
Compared with unfilled PBT, SK603 NC010 reduces mould shrinkage from approximately 1.5–2.0% to 0.3% parallel and 1.0% normal, as measured by ISO 294-4. The tensile modulus increases from approximately 2600 MPa to approximately 6800 MPa, while tensile strain at break decreases from above 20% to approximately 3.0%. The density rises from 1.31 g/cm³ to 1.45 g/cm³. Against a 30% glass-reinforced PBT compound, SK603 NC010 has lower density, lower tool abrasion, and easier filling of thin-wall sections below 1.0 mm, but lower tensile modulus and lower HDT. Table 2 summarises approximate comparative values for representative grades; exact product comparisons should be confirmed with Celanese datasheets.
| Property | SK603 NC010 PBT GF20 | Unfilled PBT representative | PBT GF30 representative |
|---|---|---|---|
| Density | 1.45 g/cm³ | 1.31 g/cm³ | 1.54 g/cm³ |
| Tensile modulus | 6800 MPa | 2600 MPa | 9500 MPa |
| Tensile strain at break | 3.0% | 20% | 2.0% |
| Notched Charpy impact | 6.0 kJ/m² | 3.0 kJ/m² | 8.0 kJ/m² |
| HDT at 1.80 MPa | 190°C | 60°C | 205°C |
| Mould shrinkage parallel | 0.3% | 1.8% | 0.2% |
SK603 NC010 is not a direct substitute for flame-retardant Crastin® grades in electrical applications requiring UL 94 V-0 at 0.75 mm or 1.5 mm. The natural grade is rated HB; flame-retardant PBT variants achieve V-0 through additive systems that usually reduce tensile strength and impact. The product is not UV-stabilized by default; outdoor exposure without carbon black or a UV stabilization package can cause surface chalking and embrittlement. Chemical resistance is typical of semi-crystalline PBT: the compound resists aliphatic hydrocarbons, alcohols, dilute acids, and many automotive fluids at room temperature, but concentrated acids, strong bases, and hot water above 80°C hydrolyze the ester groups. Continuous contact with hot ethylene glycol/water coolant above 90°C is outside the recommended service window. Under REACH Regulation (EC) No 1907/2006 and RoHS Directive 2011/65/EU, natural non-flame-retardant PBT GF20 compounds are generally compliant when supported by the supplier’s conformity statement, but the material does not automatically carry food-contact approval under FDA 21 CFR or medical certification under ISO 10993. Those end-use requirements must be confirmed in writing with Celanese for the specific moulded article and sterilization method.
Substitution of SK603 NC010 into an existing production article requires verification of the mould shrinkage class, weld-line placement, and processing-temperature limits against the previous resin. A nominal 0.3% parallel shrinkage value does not remove the need for cavity-specific capability studies, because gate location, wall thickness, and hold pressure shift the actual shrinkage range. Where the part carries an electrical insulation coordination rating under IEC 60664-1, moulded creepage distances must be measured after thermal conditioning, not on green parts. For automotive under-hood brackets, the material should be tested for heat ageing, fatigue, and chemical exposure at the actual soak temperature and fluid mixture, because published laboratory data for this specific configuration is limited above 120°C. The absence of a flame-retardant package also means that electrical products must be evaluated for end-product ignition resistance under the applicable appliance standard, since the material itself is only UL 94 HB at 1.6 mm. These boundary conditions define the usable specification window for Celanese Crastin® PBT+GF20% SK603 NC010.