| HS Code | 639979 |
| Product Name | Celanese Crastin® PBT+GF20%-FR SK643FR NC010 |
| Manufacturer | Celanese |
| Trade Name | Crastin |
| Grade | SK643FR NC010 |
| Polymer Type | PBT |
| Filler Reinforcement | 20% glass fiber |
| Flame Retardant | Yes |
| Color | Natural |
| Processing Method | Injection molding |
| Density | 1.53 g/cm³ |
| Molding Shrinkage Parallel | 0.4 % |
| Molding Shrinkage Normal | 1.0 % |
| Tensile Modulus | 7300 MPa |
| Tensile Stress At Break | 100 MPa |
| Tensile Strain At Break | 2.5 % |
| Flexural Modulus | 7000 MPa |
| Charpy Notched Impact Strength 23c | 6 kJ/m² |
| Hdt A | 205 °C |
| Hdt B | 175 °C |
| Melting Temperature | 225 °C |
| Ul94 Flammability Rating | V-0 |
| Comparative Tracking Index | 600 V |
| Volume Resistivity | >1E14 ohm·cm |
| Dielectric Strength | 30 kV/mm |
As an accredited Celanese Crastin® PBT+GF20%-FR SK643FR NC010 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Supplied in 25 kg net-weight, polyethylene-lined moisture-barrier paper bags, palletized; keep sealed in original packaging until use. |
| Container Loading (20′ FCL) | 20′ FCL container loaded with palletized 25 kg bags of Celanese Crastin® PBT+GF20%-FR SK643FR NC010, properly secured for ocean shipment. |
| Shipping | Shipping description: Celanese Crastin® PBT+GF20%-FR SK643FR NC010, glass-fiber reinforced flame-retardant PBT pellets, is not regulated as dangerous goods for road, sea, or air transport. No UN number, hazard class, or packing group. Ship in dry, sealed packaging; avoid moisture, heat, and contamination. |
| Storage | Store Celanese Crastin® PBT+GF20%-FR SK643FR NC010 in its original, sealed packaging in a cool, dry, well-ventilated area. Protect it from moisture, direct sunlight, heat and ignition sources. Keep containers closed when not in use, avoid dust generation, and prevent contact with incompatible chemicals. Follow local regulations and the product SDS for additional storage and handling requirements. |
| Shelf Life | Shelf life is typically 24 months when stored in original unopened packaging, dry, cool, and away from sunlight/moisture. |
Competitive Celanese Crastin® PBT+GF20%-FR SK643FR NC010 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Celanese Crastin® PBT+GF20%-FR SK643FR NC010 is an injection-molding grade of polybutylene terephthalate reinforced with 20% glass fibers and modified with a flame-retardant package. The NC010 designation identifies an unpigmented, natural-color feed. The grade is intended for connectors, terminal blocks, relay bases, contact carriers, switch housings, and power-distribution insulators where dimensional control after demolding and a material-level flammability classification of UL 94 V-0 at 0.75 mm are required. The fiber fraction is deliberately positioned between unfilled flame-retardant PBT and 30% glass-reinforced FR-PBT; it raises stiffness relative to unfilled grades while retaining more balanced flow and lower warpage than highly filled systems.
The glass content is not an incidental filler level. At 20% by mass, the reinforcement changes melt rheology, thermal conductivity, and mechanical anisotropy compared with unfilled PBT. In the NC010 natural grade, the absence of pigment removes one variable from flame-retardant behavior, but any later addition of color masterbatch must be validated against UL 94 performance on production-representative parts.
Published Celanese data list a density of 1.51 g/cm³ by ISO 1183, a tensile modulus of approximately 7800 MPa by ISO 527-1/-2, and tensile stress at break near 95 MPa. Elongation at break remains below 3%, which limits snap-fit deflection and makes sharp internal radii more sensitive to stress concentration than in unreinforced PBT. Charpy notched impact strength is approximately 6.0 kJ/m² by ISO 179/1eA, flexural modulus is near 6800 MPa by ISO 178, and deflection temperature under 1.8 MPa load is approximately 195 °C by ISO 75-1/-2. The melt peak by ISO 11357-3 is near 225 °C.
Mold shrinkage under ISO 294-4 is reported in the order of 0.4% in the flow direction and 1.0% transverse for standard plaques. This anisotropy must be carried into tool-making calculations; ignoring the transverse component can produce bowing in flat parts. Fiber orientation at weld lines lowers local impact strength to roughly 50% of bulk Charpy values, and gate placement should keep weld lines out of snap-fit roots or pin-retention zones.
Heat resistance should be interpreted through UL 746B Relative Temperature Index rather than HDT alone. Published data for continuous oxidative aging of this specific configuration above 130 °C are limited, and hot-water exposure above 85 °C can hydrolyze the polyester backbone. The compound is not intended for service in strong alkaline media, hot glycol-water immersion, or direct food contact without application-specific validation.
At room-temperature 50% relative humidity, PBT pellets gain moisture slowly, but once melted, the degradation pathway is autocatalytic: hydrolysis lowers molecular weight, which lowers melt viscosity, which accelerates further hydrolysis. Drying is therefore a processing boundary, not a cosmetic recommendation. Production dryers with temperature and dew-point logging are preferred over simple hot-air hoppers.
Drying is the first independent variable. PBT absorbs enough moisture at 50% relative humidity to exceed 0.05% moisture in open storage, and melt moisture above 0.02% produces splay, loss of molecular weight, and reduced weld-line strength. Closed desiccant drying at 120 °C for 4 h to 6 h with a dew point below -30 °C is mandatory. If conveying lines operate above 60% relative humidity without dry-air purge, re-adsorption can occur within 30 min. Drying above 140 °C is unnecessary and may cause additive migration to pellet surfaces.
Melt-temperature control is narrow. The preferred nozzle temperature is 250 °C to 260 °C, with metering-zone settings of 240 °C to 260 °C. Above 270 °C, thermal degradation of the flame-retardant package can release acidic decomposition products; these produce black specks, visible streaking, and corrosion of polished tool surfaces. Residence time at 260 °C should not exceed 5 min. Below 235 °C, glass bundles remain poorly dispersed and screw torque increases, leading to gate-area fiber orientation defects.
Residence-time control also depends on shot-to-barrel capacity ratio. If the shot weight is less than 25% of barrel capacity, material remains in the barrel longer and may degrade even within nominal temperature settings. For small parts below 5 g, a smaller injection unit or reduced barrel temperature is required to keep total residence time below 5 min. Purge routines with a thermally stable carrier should be established after any interruption exceeding 10 min.
Shear history is controlled with screw speed and back pressure. Screw speed between 50 min⁻¹ and 100 min⁻¹ and back pressure of 0.3 MPa to 0.5 MPa are appropriate starting values on general-purpose screws. High back pressure generates viscous heating and reduces retained fiber length, lowering notched impact. Low back pressure permits pellet-to-pellet temperature variation and air entrapment in thick sections. Injection speed should be medium-to-high for thin walls below 1.5 mm; however, excessive speed at gate lands thinner than 0.8 mm can produce shear marks and local flame-retardant degradation.
Packing pressure is typically 50 MPa to 70 MPa hydraulic, with a low-velocity pack profile to avoid overpacking near the gate. Overpacking increases flash tendency and fiber orientation stress, leading to warpage after annealing. Switch-over from injection to packing should occur before the screw reaches a cushion of 3 mm to 5 mm; a larger cushion produces inconsistent shot weights and dimensional variation.
Tool temperature is maintained at 60 °C to 90 °C. At cavity temperatures below 50 °C, the frozen skin prevents complete crystallization in the core; post-mold shrinkage of 0.2% to 0.3% can occur over 24 h. For flat connector housings longer than 80 mm, cavity-to-cavity temperature differences above 10 °C have been associated with bowing and pin-to-pin position drift. Uniform water circuits, pressure gauges in each circuit, and cavity surface probes are specified in production tool builds.
Because SK643FR NC010 solidifies rapidly, gate freeze time limits how much packing pressure can influence shrinkage. With 20% glass, flow-direction shrinkage is typically 0.3% to 0.5% for 2 mm plaques, while transverse shrinkage is 0.8% to 1.0%; this anisotropy remains even at high pack pressures if the gate freezes before the cavity center is fully packed. Edge gates or fan gates are preferred for parts longer than 40 mm. Submarine gates below 1.0 mm diameter freeze early, restrict packing, and can produce sink or warpage that is frequently misattributed to material variation.
Screw geometry further qualifies processing. A general-purpose screw with 20:1 to 25:1 L/D and compression ratio 2.5:1 to 3.0:1 is sufficient; high-shear mixing pins are not recommended because they reduce glass-fiber length and notched impact. Hot-runner systems should use powered valve gates with independent tip control because open torpedo tips create low-velocity dead zones where flame-retardant decomposition can begin. Non-return valves must be inspected for ring and seat wear; a melt cushion variation of 2 mm to 5 mm on small machines can produce dimensional drift in multi-cavity tools.
Regrind use is permitted up to 20% by mass with virgin pellets if the regrind is dried and free of fines. Higher levels can reduce impact strength and alter UL 94 performance. Regrind particle size below 4 mm disperses more uniformly than large sprues above 8 mm. Fines above 0.5% by mass can create surface pitting and gas splay.
Black specks in molded parts are most often generated by thermal degradation of the flame-retardant package in the screw channel or hot-runner dead spot, not by contaminated pellets. If black specks appear, the first correction is to lower the nozzle and manifold temperatures by 5 °C to 10 °C and reduce screw speed, rather than increasing purge frequency alone. Surface splay indicates either wet pellets or unmelted glass-fiber bundles; the two can be distinguished by moisture analysis of the feed.
The following values are typical, not specification minima, and refer to unpigmented NC010 molded under the conditions described above.
| Property or classification | Standard | Typical value or condition |
|---|---|---|
| Flammability | UL 94 | V-0 at 0.75 mm and 1.5 mm |
| Glow-wire flammability index | IEC 60695-2-12 | 960 °C at 2.0 mm |
| Glow-wire ignition temperature | IEC 60695-2-13 | 775 °C at 2.0 mm |
| Comparative tracking index | IEC 60112 | 250 V |
| Tensile modulus | ISO 527-1/-2 | 7800 MPa |
| Flexural modulus | ISO 178 | 6800 MPa |
| Charpy notched impact strength | ISO 179/1eA | 6.0 kJ/m² |
| Heat deflection temperature | ISO 75-1/-2 | 195 °C at 1.8 MPa |
The 960 °C glow-wire value supports end-product testing under IEC 60335-2-30, but the material classification does not automatically confer compliance on a finished component. Color masterbatches, metal inserts, weld lines, gate vestiges, and unvented blind holes can reduce glow-wire performance and must be evaluated on production-representative parts. The comparative tracking index of 250 V is relevant for creepage-distance calculations under IEC 60664-1; it is not applicable without additional surface protection in pollution degree 4 environments or where conductive dust can bridge narrow gaps.
In relay bases and terminal blocks, the combination of UL 94 V-0 at 0.75 mm and 250 V CTI supports compact thin-wall designs. The glass-reinforced grade provides lower creep under contact insertion force than unfilled PBT, but insert design must avoid sharp corners because the low elongation at break makes the material notch-sensitive. Ultrasonic welding is possible, but weld strength is reduced by the glass-fiber content compared with unfilled PBT; hot-plate welding is preferred for structural joints.
Compared with an unfilled flame-retardant PBT, SK643FR NC010 raises tensile modulus from approximately 2800 MPa to 7800 MPa and reduces flow-direction mold shrinkage from approximately 1.5% to 0.4% in a 2 mm plaque. The trade-off is reduced elongation at break, from above 8% to below 3%, and a density increase of roughly 5% to 8%, which may raise part mass and cycle time. Against a 30% glass-filled FR-PBT, this grade has lower flexural modulus but lower warpage in flat ribbed designs and better thin-wall flow. The 20% reinforcement level is therefore suited to connectors where pin-position tolerance and flatness after demolding dominate over maximum load-bearing capability.
Against a 30% glass-reinforced FR-PBT, SK643FR NC010 also differs in melt viscosity. Published data for this specific configuration is limited, but the lower fiber loading gives lower apparent melt viscosity and permits longer flow length in spiral-flow molds at equivalent melt temperature. This is useful for thin-wall connector housings below 1.2 mm, where the 30% grade may short-shot before filling finishes.
Water absorption of glass-reinforced PBT is approximately 0.3% by ISO 62 after 24 h immersion. Although short-term dimensional change is generally below 0.1%, repeated humidity cycles relax molded-in stresses and can release anisotropic shrinkage. Parts that measure within 0.05 mm after molding may deviate beyond tolerance after 50 cycles between 25 °C and 85 °C at 85% relative humidity if gates were undersized or packing time was held too short.
Dielectric strength on dry specimens is reported above 20 kV/mm by IEC 60243-1. At 80% relative humidity, surface resistivity can decrease by two orders of magnitude relative to conditioned values, although volume resistivity is less affected. Creepage surfaces on rib roots and boss bases therefore require design review in humid switchgear; the behavior is common to glass-filled PBT and is not limited to one flame-retardant package.
Storage life in sealed bags at 23 °C and 50% relative humidity is typically 24 months from the date of certification. Even within this period, drying before molding remains mandatory. Material declarations should be verified against current REACH and RoHS lists, and end-product requirements under EU 2019/2021 or relevant electrotechnical directives must be assessed separately. Published data for this specific configuration under outdoor UV aging is limited, and the grade should not be exposed to direct sunlight in applications without a UV-stabilized housing or coating.
Mold-filling simulations for SK643FR NC010 should not use unfilled PBT viscosity or shrinkage data. The glass-fiber fraction raises thermal conductivity and accelerates freeze-off at the flow front; walls below 0.8 mm require high injection speed and tool temperatures near 90 °C to avoid short shots. The flame-retardant package also narrows the thermal window relative to general-purpose PBT, so production controls should log melt temperature, residence time, and material moisture at the press rather than treating them as secondary settings.