| HS Code | 482309 |
| Material Type | Polybutylene terephthalate (PBT) with 15% glass fiber |
| Color | Natural |
| Density | 1.41 g/cm3 |
| Glass Fiber Content | 15% |
| Tensile Modulus | 5500 MPa |
| Tensile Stress At Break | 100 MPa |
| Tensile Strain At Break | 2.5% |
| Charpy Notched Impact Strength At 23 C | 5 kJ/m2 |
| Melting Temperature | 225 °C |
| Heat Deflection Temperature At 1 8 Mpa | 200 °C |
| Molding Shrinkage Parallel | 0.4% |
| Molding Shrinkage Normal | 1.0% |
| Water Absorption After 24 H | 0.2% |
| Volume Resistivity | >1E14 ohm·cm |
| Flammability | HB |
As an accredited Celanese Crastin® PBT+GF15% SK602 NC010 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaged in 25 kg moisture-barrier bags, Celanese Crastin® PBT+GF15% SK602 NC010 supplied as natural-color pellets for injection molding. |
| Container Loading (20′ FCL) | A 20′ FCL container loaded with palletized 25 kg bags of Celanese Crastin® PBT+GF15% SK602 NC010, secured for transport. |
| Shipping | Celanese Crastin® PBT+GF15% SK602 NC010 is a 15% glass-fiber-reinforced polybutylene terephthalate resin supplied as natural-color pellets in moisture-barrier bags or sealed containers. It is non-hazardous for transport, should be kept dry, cool, and protected from UV/contamination, and shipped under standard freight conditions. |
| Storage | Store in a cool, dry, well-ventilated area away from direct sunlight, heat, flames, and ignition sources. Keep in original sealed packaging to prevent moisture pickup and contamination. Avoid prolonged exposure to humid conditions; reseal opened bags and use desiccant if recommended. Do not store outdoors or near oxidizing materials. Ensure containers remain closed and labeled, and follow local regulations. |
| Shelf Life | Shelf life is 2 years from date of manufacture when stored in original unopened packaging at temperatures not exceeding 30°C. |
Competitive Celanese Crastin® PBT+GF15% SK602 NC010 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
The product Celanese Crastin® PBT+GF15% SK602 NC010 is classified under ISO 1043 as PBT-GF15: a polybutylene terephthalate injection moulding compound containing a nominal glass-fibre loading of 15% by weight. The NC010 suffix identifies natural uncoloured pellet supply. The material is intended for reciprocating screw injection moulding, and it is commonly processed with a general-purpose screw having an L/D ratio of 20:1 to 24:1 and a compression ratio of approximately 2.5:1. Manufacturer-recommended drying uses a desiccant dryer at 120°C for 4 h with a dew point of -30°C or lower; residual moisture before melt processing is specified below 0.02%. Barrel temperature settings should produce a melt temperature of 250°C to 270°C, while mould temperature is maintained between 60°C and 100°C. Because the terephthalate ester repeating unit is susceptible to hydrolysis, any combination of elevated moisture and excessive barrel residence time reduces molecular weight and weld-line strength.
Specification values for this grade are generated on injection moulded specimens conditioned for 48 h at 23°C and 50% relative humidity. Density according to ISO 1183-1 is approximately 1.41 g/cm³. Melt volume-flow rate is measured per ISO 1133-1 at 250°C under a 2.16 kg load, and glass-fibre content is verified by ashing according to ISO 3451-1. Tensile modulus and tensile stress at break are evaluated by ISO 527-2/1A; flexural properties are measured by ISO 178. Heat deflection temperature is determined under 1.8 MPa and 0.45 MPa by ISO 75-1/-2. Impact resistance is reported as notched Charpy per ISO 179/1eA. These are typical values and are not minimax limits; the current manufacturer technical datasheet governs.
| Property | Standard method | Test condition |
|---|---|---|
| Density | ISO 1183-1 | 23°C, immersion |
| Tensile modulus / stress | ISO 527-2/1A | Type 1A, 5 mm/min |
| Flexural modulus / stress | ISO 178 | 80 mm × 10 mm × 4 mm, 2 mm/min |
| Notched Charpy impact | ISO 179/1eA | 23°C, notch type A |
| Heat deflection temperature | ISO 75-1/-2 | 1.8 MPa, flatwise |
| Melt volume-flow rate | ISO 1133-1 | 250°C, 2.16 kg |
| Water absorption | ISO 62 | 23°C, 50% RH |
| Glass-fibre content | ISO 3451-1 | Ashing |
Selection of Crastin® SK602 NC010 instead of unfilled PBT or a 30% glass-fibre Crastin® grade is determined by the balance among stiffness, flow length, and moulded-part distortion. At 15% glass content, the compound retains lower melt viscosity than 30% glass-fibre PBT at injection shear rates, permitting the filling of connector walls below 1 mm with moderate packing pressure. The tensile modulus of a 15% glass-fibre PBT is higher than unfilled PBT and lower than a 30% glass grade; representative tensile modulus values for this product class fall between 5,000 MPa and 6,000 MPa per ISO 527-2/1A. Shrinkage measured per ISO 294-4 is anisotropic because fibres orient in the flow direction, producing lower flow-direction shrinkage than cross-flow shrinkage. The difference is smaller than that of a 30% glass grade, which reduces bowing tendency on flat parts. Creep resistance and short-term heat deflection temperature remain below those of 30% glass-fibre PBT, so a heavily loaded bracket should not be substituted into a 30% glass grade without verifying deformation at the service temperature.
Fluidity comparisons should not be made using melt volume-flow rate alone. MVR is measured at low shear by ISO 1133-1 and cannot predict high-shear mould filling. Spiral-flow tests or capillary rheometry are employed for thin-wall filling analysis. At equivalent melt temperature and injection pressure, flow length for SK602 NC010 is shorter than unfilled PBT and longer than 30% glass-fibre PBT. This property supports the filling of multi-cavity connector tools where a 30% glass grade may require higher melt temperature or additional gates. Weld-line strength is a limitation: because glass fibres do not cross the knit line, tensile strength at a weld line may be 50–70% of the bulk value. Gate placement for load-bearing connector structures should avoid knit lines in high-stress retention features.
Hydrolytic degradation of PBT proceeds through chain scission of the ester linkage and is accelerated by residual moisture and melt temperature. The 0.02% moisture limit is a feed-port requirement, not a long-term storage target. At relative humidity near 60%, natural NC010 pellets can exceed the limit within a few hours and should be re-dried before use. Desiccant-wheel dryers should deliver air at 120°C and maintain a dew point of -30°C or lower; hopper residence time should not exceed 8 h at temperature because natural pellets may oxidize and shift colour. The melt residence time should remain below 15 min at temperatures above 250°C. When production is interrupted for 15 min or longer, purging is required before restart. The use of acidic flame-retardant additives should be evaluated because acidic species can accelerate hydrolysis and reduce surface quality. Amine-based additives or uncured epoxy masterbatches should also be avoided because interactions with the ester matrix can alter crystallization kinetics.
On production lines, shot size should occupy 30% to 70% of the injection unit capacity. Back pressure between 0.3 MPa and 0.7 MPa hydraulic and screw speeds of 50 rpm to 100 rpm are typical starting values. Nozzle melt temperature should not exceed 275°C because thermal degradation produces volatile by-products that can leave residue in the mould. For hot-runner systems, manifold and nozzle set points are held at 250°C to 265°C, and the drop tip should be protected from overheating during cycle interruptions. Regrind addition above 20% is not recommended for tensile or impact-critical parts because repeated processing reduces fibre length and lowers notched impact.
| Parameter | Set point or range |
|---|---|
| Pre-drying | 120°C, 4 h, desiccant dryer, dew point ≤ -30°C |
| Residual moisture | ≤ 0.02% |
| Melt temperature | 250–270°C |
| Mould temperature | 60–100°C |
| Hot-runner temperature | 250–265°C |
| Back pressure | 0.3–0.7 MPa hydraulic |
| Screw speed | 50–100 rpm |
| Holding pressure | 60–80% of injection pressure |
| Shot size | 30–70% of injection unit capacity |
Automotive under-hood components expose the material to oils, coolants, fuels, and thermal cycling. Compatibility with engine oil, automatic transmission fluid, and unleaded fuel is generally acceptable for short-term or occasional contact below 120°C, but continuous immersion in glycol-based coolant at elevated temperature can reduce glass-fibre adhesion and produce surface fibre prominence. Direct contact with hot water above 60°C or with steam is outside the recommended service envelope because ester hydrolysis progressively reduces impact strength. Strong alkaline media attack the terephthalate ester and are not recommended. For enclosed electrical modules with low-outgassing requirements, melt temperature should be controlled below 270°C because PBT thermal degradation can generate tetrahydrofuran and other volatile species. Published single-chemical compatibility data for this exact grade is limited; new applications require immersion testing according to ISO 175 or an equivalent customer specification.
Thermal ageing resistance is assessed by accelerated air-oven ageing according to ISO 188 or by long-term thermal rating per UL 746B. The manufacturer’s UL Yellow Card provides the relative thermal index for the grade; this value is thickness- and formulation-dependent and should not be inferred from heat deflection temperature alone. The grade is normally rated UL 94 HB at standard thicknesses; if a V-0 flammability classification is required, a flame-retardant glass-reinforced PBT grade should be selected because adding flame-retardant masterbatch to a natural HB grade may alter tracking resistance and mechanical properties.
Electrical connector and sensor housing applications benefit from lower moisture absorption than PA66. Equilibrium water absorption at 23°C and 50% relative humidity for glass-reinforced PBT is typically below 0.2% per ISO 62, whereas PA66 absorbs several times that amount. Dielectric strength is measured on 2 mm plaques according to IEC 60243-1; comparative tracking index is measured by IEC 60112. The CTI value for natural SK602 NC010 should be taken from the UL Yellow Card because mould-release residues, pigmentation, and regrind content influence surface tracking behaviour. For high-voltage spacing, surface contamination must be controlled through cleaning and handling procedures because tracking resistance is a surface phenomenon.
Linear thermal expansion of glass-reinforced PBT is anisotropic: flow-direction coefficient of linear thermal expansion is lower than cross-flow because glass fibres constrain expansion. For design calculations, values determined by ISO 11359-2 on specimens cut parallel and perpendicular to flow should be used. The glass transition temperature of PBT is near 45–60°C; above this region, modulus decreases and creep rate increases. Electrical connectors that experience continuous load at high temperature may deform unless brass or steel terminals provide mechanical support. The short-term heat deflection temperature under 1.8 MPa is not a continuous-use temperature.
Mould temperature influences crystallization, surface appearance, and shrinkage. At the lower end of the recommended range, the surface may have low gloss and the part may exhibit higher post-mould shrinkage. At the upper end, crystallization is more complete, reducing post-mould shrinkage and improving dimensional stability but increasing cycle time. For critical dimensional applications, a mould temperature of 80°C to 100°C is preferred. Differential scanning calorimetry shows that PBT crystallization occurs rapidly, permitting short holding times, but gate freeze must be confirmed by gate-freeze studies using cavity-pressure sensors.
Warpage control in SK602 NC010 parts depends on gate geometry, packing profile, and cooling uniformity. Fibre orientation is highest near the mould surface and lower in the core. An edge gate creates strong flow-direction orientation and may produce bowing in flat housings; a centre sprue or diaphragm gate yields more axisymmetric orientation and less distortion. Cavity surface temperature variation should be maintained within ±5°C across the part because differential crystallization shrinkage can dominate fibre orientation effects in thicker sections. Tool vents should be placed at knit lines and last-filled areas to prevent diesel burns in natural NC010. If post-mould warpage is observed, increasing mould temperature and adjusting holding pressure are preferred over extending packing time, which can increase gate-area stress and visible gate blush.
Natural NC010 pellets should be kept sealed in moisture-barrier packaging until use. After opening, exposed material should be consumed within the shift or re-dried. Conveying systems should be clean to avoid contamination from polyamide or acetal, which can cause delamination or colour contamination. Regrind should be collected and dried under the same conditions; contamination from oil mist, mould release, or paper labels must be excluded.
Relative to PBT/PET blends, SK602 NC010 offers faster crystallization and lower mould temperature requirements, which can shorten cooling time in thick sections. Relative to PA66, the grade provides more stable dielectric and mechanical dimensions in humid environments but lower dry-as-moulded impact and lower continuous heat resistance. Relative to higher-glass PBT grades, the 15% product improves flow and reduces anisotropic shrinkage while sacrificing some modulus and creep resistance. These differences are the primary design inputs when selecting among engineering thermoplastics for precision electrical connectors, switches, bobbins, and sensor housings.
Compliance documentation may be requested under REACH Regulation (EC) No 1907/2006 and the EU RoHS Directive 2011/65/EU. The material is supplied under the manufacturer’s standard quality system; customers requiring controlled lot release and full traceability should specify these requirements at order entry. The grade is not intended for food-contact, pharmaceutical, or implantable medical use unless migration testing is completed for the intended application. No statement in this document substitutes for the latest manufacturer material datasheet or UL certification.