| HS Code | 440737 |
| Density | 1.54 g/cm³ |
| Glass Fiber Content | 15% |
| Tensile Modulus | 5500 MPa |
| Tensile Stress At Break | 95 MPa |
| Elongation At Break | 2.5% |
| Charpy Notched Impact Strength | 5 kJ/m² |
| Charpy Unnotched Impact Strength | 30 kJ/m² |
| Heat Deflection Temperature At 0 45 Mpa | 205 °C |
| Heat Deflection Temperature At 1 8 Mpa | 185 °C |
| Melting Temperature | 225 °C |
| Flammability Rating Ul94 | V-0 at 0.75 mm |
| Glow Wire Flammability Index | 960 °C at 0.75 mm |
| Comparative Tracking Index | 350 V |
| Water Absorption | 0.1% |
| Mold Shrinkage Parallel | 0.4% |
| Mold Shrinkage Normal | 0.9% |
As an accredited Celanese Crastin® PBT+GF15%-FR CE15315 BK010 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaged as 25 kg moisture-barrier bags, palletized and labeled, for Celanese Crastin® PBT+GF15%-FR CE15315 BK010 industrial resin handling. |
| Container Loading (20′ FCL) | 20′ FCL container loading: palletized 25 kg bags of Celanese Crastin® PBT+GF15%-FR CE15315 BK010, full container load, secure and dry. |
| Shipping | Celanese Crastin® PBT+GF15%-FR CE15315 BK010 is supplied as black, 15% glass-fiber reinforced, flame-retardant PBT pellets in moisture-proof sealed bags or octabins on pallets. Ship under dry, cool conditions, avoiding humidity, heat, and UV exposure; generally non-hazardous for transport. |
| Storage | Store Celanese Crastin® PBT+GF15%-FR CE15315 BK010 in a cool, dry, well-ventilated area away from direct sunlight, heat, flames, and ignition sources. Keep containers tightly closed to prevent moisture ingress and contamination. Avoid contact with strong oxidizing agents and incompatible chemicals. Maintain good housekeeping to control dust and follow local safety and environmental regulations. |
| Shelf Life | Shelf life is typically 24 months when stored unopened in original packaging in a dry, cool place. |
Competitive Celanese Crastin® PBT+GF15%-FR CE15315 BK010 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Celanese Crastin® PBT+GF15%-FR CE15315 BK010 is an injection-moulding compound based on polybutylene terephthalate containing 15 wt% short-glass fibre and a flame-retardant additive package, supplied as black pellets under the BK010 colour designation. The grade is positioned for electrical insulation, connector, switch, sensor, and appliance housing components that require a UL 94 vertical burning classification of V-0 at thin wall thickness. Published property data are generated according to ISO 1183-1, ISO 527-1/-2, ISO 178, ISO 179/1eA, ISO 75-2, and ISO 1133-1. Lot-specific values are traceable through the manufacturer certificate of analysis, and the current UL yellow card remains the authoritative source for flame-retardant classifications.
The polymer matrix is semicrystalline PBT, which crystallizes rapidly during cooling from the melt. The 15 wt% short-glass reinforcement disperses in the melt under normal injection-moulding shear and produces a mechanical response between unfilled PBT and higher-glass-loading PBT grades. Published tensile modulus for Crastin® CE15315 BK010 is approximately 7,000 MPa under ISO 527-2/1A, compared with approximately 2,600 MPa for unfilled PBT and approximately 5,500 MPa for a similar non-flame-retardant PBT-GF15 compound. Tensile strain at break is reduced to approximately 2.0% to 2.8%, reflecting the stiffening effect of the fibre network.
The glass network also lowers mould shrinkage from the 1.8% to 2.2% typical of unfilled PBT to approximately 0.4% to 0.6% in the flow direction and 0.8% to 1.1% transverse to flow, measured after 24 h at 23°C and 50% relative humidity under ISO 294-4. Because fibre orientation follows the melt front, the compound is anisotropic; weld-line strength can be lower than bulk strength by 20% to 40% depending on part geometry, gate location, and melt temperature. The flame-retardant package reduces impact toughness relative to non-FR PBT-GF15. Published Charpy notched impact strength for CE15315 BK010 is in the 6.5 kJ/m² to 8.5 kJ/m² range under ISO 179/1eA, placing the grade in the medium-toughness class for glass-filled polyester. Design with sharp internal corners or weld lines in load-bearing areas should therefore be avoided unless verified by part testing. The grade is classified as PBT-GF15-FR under ISO 1043-1.
Moisture control is the first operational boundary. PBT absorbs less water than aliphatic polyamides, but hydrolytic degradation of ester linkages occurs when residual moisture exceeds 0.02 wt% measured by ISO 15512. Desiccant drying at 120°C for 4 h is normally required; at storage relative humidity above 60%, drying time should be extended to 6 h. The dryer dew point should remain at −40°C or lower, with minimum airflow of 0.4 m³/h per kg of resin throughput. Barrel temperature profiles are conventionally staged from 240°C in the feed zone to 260°C at the nozzle, with the melt temperature measured between 245°C and 270°C. Residence time above 285°C should be limited to less than 5 min because PBT degrades through ester scission and tetrahydrofuran formation; prolonged thermal exposure reduces melt viscosity and tensile properties.
A general-purpose injection-moulding screw with L/D 20:1 to 22:1 and compression ratio 2.5:1 to 3.0:1 is suitable. Compression ratios above 3.5:1 can generate excessive shear heating in a glass-filled compound and reduce mean fibre length. Back pressure between 2 MPa and 5 MPa maintains melt homogeneity without overworking the fibre. Injection velocity is selected according to flow length/wall thickness ratio; thin-wall connectors with ratios above 100 commonly require injection velocities up to 150 mm/s. Hold pressure is set between 40% and 60% of peak injection pressure to control sink and achieve part mass stability. Mould temperature is maintained between 60°C and 100°C; the upper end improves crystallinity and reduces post-mould dimensional change, but increases cycle time. Regrind use should not exceed 20 wt% when the regrind is properly dried, free of contamination, and uniformly granulated; higher regrind fractions reduce impact strength and may shift UL 94 performance.
Flame-retardant behaviour and electrical insulation characteristics for CE15315 BK010 are evaluated under the vertical burning protocols of IEC 60695-11-10 and UL 94. The published UL yellow-card classification for this grade is V-0 at 0.8 mm and 1.6 mm nominal thickness. Applications in unattended appliance components also require glow-wire test data; the glow-wire flammability index is typically reported as 960°C at 1.0 mm under IEC 60695-2-12, and the glow-wire ignition temperature as 775°C at 1.0 mm under IEC 60695-2-13. The comparative tracking index is reported as 600 V under IEC 60112, indicating resistance to conductive bridging in polluted environments. Short-term electric strength for glass-reinforced FR PBT is normally in the range of 20 kV/mm to 30 kV/mm under IEC 60243-1, but component geometry, electrode type, and wall thickness influence the final insulation performance. These data support use in relay bases, coil formers, motor end caps, switch housings, and connector bodies where the part must survive both overcurrent-generated heat and electrical tracking across creepage distances.
| Property | Test method | Published value or range |
|---|---|---|
| Density | ISO 1183-1 | 1.54–1.56 g/cm³ |
| Tensile modulus | ISO 527-2/1A | 6,900–7,400 MPa |
| Tensile stress at break | ISO 527-2/1A | 95–110 MPa |
| Tensile strain at break | ISO 527-2/1A | 2.0–2.8% |
| Flexural modulus | ISO 178 | 6,000–6,600 MPa |
| Flexural strength | ISO 178 | 145–165 MPa |
| Charpy notched impact strength | ISO 179/1eA | 6.5–8.5 kJ/m² |
| Charpy unnotched impact strength | ISO 179/1eU | 35–45 kJ/m² |
| Melt volume-flow rate | ISO 1133-1, 250°C/2.16 kg | 14–18 cm³/10 min |
| Heat deflection temperature HDT/A | ISO 75-2, 1.8 MPa | 185–195°C |
| Flame retardance | UL 94/IEC 60695-11-10 | V-0 at 0.8 mm |
| Water absorption, saturation | ISO 62 | 0.3–0.5% |
| Mould shrinkage, parallel | ISO 294-4 | 0.4–0.6% |
| Mould shrinkage, perpendicular | ISO 294-4 | 0.8–1.1% |
Operational boundaries include continuous use temperature indexed by UL 746B relative temperature index. RTI values for glass-filled flame-retardant PBT are commonly reported as 130°C for electrical, mechanical, and impact retention at 0.8 mm; the exact RTI for CE15315 BK010 must be confirmed on the current UL yellow card. Prolonged contact with hot water above 60°C, strong acids, strong alkaline solutions, or coolants maintained outside a pH range of 5 to 8 promotes polyester hydrolysis. The grade is therefore not appropriate for applications requiring sustained exposure to pressurised hot-water extraction or aggressive chemical cleaning. Flame-retardant additive packages can generate plate-out on tool surfaces during extended production runs; venting and periodic tool maintenance should be scheduled. When recompounding with post-industrial scrap or masterbatch, laboratory compounding on a 40:1 L/D twin-screw extruder with zone temperatures of 240°C to 260°C is used to detect additive antagonism before production scale-up. Published data for specific combinations with certain nucleating agents or amine-based stabilizers are limited; compatibility must be verified experimentally.
Selecting CE15315 BK010 over unfilled, non-flame-retardant PBT changes the design envelope in measurable ways. Density rises from approximately 1.31 g/cm³ to approximately 1.55 g/cm³ under ISO 1183-1, which is a boundary condition for lightweighting. The tensile modulus increase to approximately 7,000 MPa allows thinner structural sections in non-load-bearing electrical housings, but impact toughness remains below that of ductile unfilled PBT. Compared with non-FR PBT-GF15, the FR package reduces notched impact strength by approximately 10% to 20% and may narrow the melt-processing window slightly. Compared with higher-glass PBT-GF30 halogenated FR compounds, CE15315 BK010 typically offers lower density, lower melt viscosity, and better thin-wall flow at the same mould temperature, but lower tensile modulus and flexural strength. The 15 wt% glass content represents a middle position between unfilled FR PBT and 30 wt% glass formulations.
| Property | Unfilled PBT | PBT-GF15 non-FR | CE15315 BK010 | PBT-GF30 FR |
|---|---|---|---|---|
| Density, ISO 1183-1 | 1.31 g/cm³ | 1.44 g/cm³ | 1.55 g/cm³ | 1.65 g/cm³ |
| Tensile modulus, ISO 527-2/1A | 2,600 MPa | 5,500 MPa | 7,000 MPa | 9,000 MPa |
| Heat deflection temperature, ISO 75-2, 1.8 MPa | 55°C | 200°C | 190°C | 205°C |
| Flame retardance, UL 94 | HB | HB | V-0 at 0.8 mm | V-0 at 0.8 mm |
| Mould shrinkage, parallel, ISO 294-4 | 1.8–2.2% | 0.5–0.7% | 0.4–0.6% | 0.3–0.5% |
| Charpy notched impact, ISO 179/1eA | 3–4 kJ/m² | 8–10 kJ/m² | 6.5–8.5 kJ/m² | 8–10 kJ/m² |
These class-level comparisons are not a substitute for lot-specific data or application testing. Selection between CE15315 BK010 and PBT-GF30 FR is often controlled by flow-length requirements, tool wear limits, and mechanical demands. In multi-cavity tools with small gates, the lower glass content of CE15315 BK010 reduces pressure drop and may permit lower clamp force on a given projected area. In parts with high creep resistance, the higher fibre content of 30 wt% grades provides greater room-temperature and elevated-temperature modulus. The product also differs from many unhalogenated PBT-PET blends in that the semicrystalline PBT matrix retains faster crystallization and lower moisture sensitivity than PET-containing compounds, but the exact chemical character of the flame-retardant package should be reviewed against end-user restricted substance lists such as RoHS 2011/65/EU, REACH, and the relevant IEC material declaration requirements.
Production-scale observations on black PBT-GF15-FR compounds indicate that apparent melt viscosity drift of more than 5% across an 8 h shift is associated with moisture intrusion, excessive barrel residence time, or check-ring wear. Process controllers should verify melt flow rate under ISO 1133-1 before attributing dimensional variation to tooling. Screw and barrel wear in 15 wt% glass compounds is lower than in 30 wt% glass compounds, but clearance checks against the screw manufacturer’s wear limits remain necessary at scheduled maintenance intervals. Hot-runner tip temperatures above 285°C produce decomposition plate-out and black specks, which are detectable by visual inspection and part weight stability.