Celanese Crastin Lw Pbt Lw9020 Nc010

Celanese Crastin® LW PBT LW9020 NC010

    • Product Name: Celanese Crastin® LW PBT LW9020 NC010
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 293156
    Product Name Celanese Crastin LW PBT LW9020 NC010
    Polymer Type PBT
    Reinforcement 20% glass fiber
    Color Natural
    Density 1.46 g/cm3
    Molding Shrinkage Parallel 0.3%
    Molding Shrinkage Normal 0.9%
    Tensile Modulus 7200 MPa
    Tensile Stress At Break 125 MPa
    Elongation At Break 2.5%
    Charpy Notched Impact Strength At 23 C 5.5 kJ/m2
    Hdt A At 1 8 Mpa 205 °C
    Melting Temperature 225 °C
    Water Absorption 0.4%
    Processing Method Injection molding

    As an accredited Celanese Crastin® LW PBT LW9020 NC010 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing Celanese Crastin® LW PBT LW9020 NC010 is supplied in 25 kg moisture-resistant bags, typically 40 bags per pallet.
    Container Loading (20′ FCL) Celanese Crastin® LW PBT LW9020 NC010: 20′ FCL loading, palletized 25 kg bags, up to 20 metric tons per container.
    Shipping Celanese Crastin® LW PBT LW9020 NC010 is a glass-fiber-reinforced PBT thermoplastic resin supplied in pellet form. It is not classified as dangerous for transport and may be shipped as general non-hazardous cargo in dry, clean, sealed packaging, protected from moisture, heat, and contamination. Store cool and dry.
    Storage Store Celanese Crastin® LW PBT LW9020 NC010 in a cool, dry, well-ventilated area, away from direct sunlight, heat, ignition sources, moisture, and oxidizing materials. Keep original packaging tightly closed and undamaged, on pallets, indoors. Avoid prolonged humid exposure and contamination. Maintain ambient conditions, follow first-in/first-out, and consult the Celanese SDS/technical datasheet for specific limits.
    Shelf Life Celanese Crastin LW PBT LW9020 NC010 typically has a two-year shelf life from delivery when stored dry and in unopened original packaging.
    Free Quote

    Competitive Celanese Crastin® LW PBT LW9020 NC010 prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    Celanese Crastin® LW PBT LW9020 NC010 is a semi-crystalline polyester injection-molding grade based on polybutylene terephthalate with a low-warpage filler package at a nominal loading of 20%. The LW designation indicates the low-warpage modification; the NC010 suffix denotes natural, uncolored pellets. The product is intended for rigid, dimensionally critical components in which anisotropic shrinkage, bowing, and post-mold distortion must be controlled across a multi-cavity tool.

    Mechanical values are determined on injection-molded specimens at 23°C and 50% relative humidity. Under ISO 527-1/-2, tensile modulus is 4,700 MPa, tensile stress at break is 90 MPa, and tensile strain at break is 3.6%. Flexural modulus under ISO 178 is 4,100 MPa. Notched Charpy impact under ISO 179/1eA at 23°C is 4.5 kJ/m². Density under ISO 1183-1 is 1.42 g/cm³. These values place the material near conventional 20% glass-fiber PBT in stiffness while the filler system is selected to reduce part distortion.

    Under ISO 294-4, longitudinal molding shrinkage at a 2.0 mm wall thickness and 80°C mold temperature is typically below 0.5%; transverse shrinkage is below 1.0%. The difference between the two directions is smaller than that of a conventional glass-fiber-reinforced PBT of the same nominal filler loading. This reduction in shrinkage anisotropy is the principal technical distinction of the LW9020 grade.

    The nominal filler loading is 20% by mass. Because the filler package includes low-warpage components, bulk density and flow behaviour differ from simple glass-fiber-reinforced PBT. Melt viscosity data under ISO 1133-1 or capillary rheometry should be used for mold-filling simulation; the datasheet single-point value alone is not adequate for complex multi-gate tools.

    How does the low-warpage filler package alter shrinkage anisotropy?

    In glass-fiber-reinforced PBT, fiber orientation along the flow direction produces low longitudinal shrinkage and much higher transverse shrinkage. A conventional GF20 PBT may show flow-direction shrinkage of 0.3% and transverse shrinkage above 1.0%; the resulting internal strain can bow flat parts after ejection. The low-warpage filler package in LW9020 NC010 reduces this orientation effect by modifying filler geometry. The exact filler composition is not published, but the engineering result is measured as a lower ratio of transverse to longitudinal shrinkage under ISO 294-4 and as reduced warpage in flat-panel fixtures.

    Warpage in a molded part is not controlled by material alone. Gate location, cavity filling pattern, cooling uniformity, and part thickness each influence fiber orientation and crystallization. Balanced filling is required to keep the shrinkage vector field symmetrical. Center gates, fan gates, or multiple gates are preferred when the part has a flat sealing surface. Edge gating a flat rectangular part creates a strong orientation gradient and can reintroduce bowing even with a low-warpage material.

    Table 1 compares typical published values for natural-grade LW9020 NC010 with general ranges for unfilled PBT and conventional GF20 PBT. The unfilled and conventional GF20 ranges are not grade-specific but represent typical values reported under the indicated standards.

    Property Test standard LW9020 NC010 typical Unfilled PBT typical range Conventional GF20 PBT typical range
    Density ISO 1183-1 1.42 g/cm³ 1.30–1.32 g/cm³ 1.44–1.46 g/cm³
    Tensile modulus ISO 527-1/-2 4,700 MPa 2,500–2,800 MPa 4,500–5,500 MPa
    Tensile strain at break ISO 527-1/-2 3.6% 50–200% 2.5–4.0%
    Flexural modulus ISO 178 4,100 MPa 2,200–2,500 MPa 4,000–5,000 MPa
    Notched Charpy impact ISO 179/1eA 4.5 kJ/m² 3.0–4.0 kJ/m² 4.0–6.0 kJ/m²
    Parallel mold shrinkage ISO 294-4 <0.5% 1.5–2.0% 0.3–0.5%

    Compared with unfilled PBT, the tensile modulus of LW9020 NC010 is approximately 88% higher and parallel mold shrinkage is more than 70% lower. Compared with conventional GF20 PBT, the trade-off is usually a small reduction in notched impact and melt flow in exchange for lower distortion in flat parts. The material is not a flame-retardant compound and is not intended for hot-water structural service; flame-retardant and hydrolysis-resistant grades must be selected where those conditions apply.

    Processing conditions that govern crystallinity and post-mold shrinkage

    Drying is mandatory before melt processing. PBT undergoes hydrolytic chain scission when moisture is present at melt temperature. The pellets should be dried at 120°C for 4 h in a desiccant dryer with a dew point of -40°C or lower, until residual moisture is below 0.02% by Karl Fischer titration. Hopper residence time should be short; insulated hoppers with dry-air purge are used on production lines to prevent moisture regaining between drying and feed throat.

    Melt temperature should be held at 250–270°C, verified by air-shot pyrometry. Barrel settings are typically rear 240–250°C, center 250–260°C, front 255–265°C, and nozzle 260–270°C. Melt temperatures above 280°C accelerate thermal degradation, leading to yellowing, melt-viscosity loss, and reduced weld-line strength. Mold temperature is controlled at 60–100°C; 80°C is the standard starting point for dimensional stability, while 90–100°C may improve crystallinity in walls below 1.0 mm.

    Injection speed should be high enough to fill before freeze-off but not so high that jetting or shear-induced filler separation occurs. Packing pressure is typically 50–80% of peak injection pressure, and gate-freeze time should be confirmed by cavity-pressure measurement or sequential short-shot testing. Back pressure of 0.3–0.7 MPa and screw rotation of 50–100 min⁻¹ are typical starting points for glass-filled PBT; machine-specific settings must be optimized with actual tooling.

    The screw and barrel should be wear-resistant because glass-fiber filler is abrasive. Screw L/D of 18:1 to 24:1 with a compression ratio of 2:1 to 3:1 is common. Melt residence time should be kept below 5 min at temperature. During brief interruptions, the screw should retract and the melt cushion should be small; for longer stops, purging with a clean PBT or purging compound is necessary. Hot-runner manifolds should be held at 250–270°C, and dead spots that allow polymer stagnation must be eliminated. Shut-off nozzles reduce drool at the sprue and prevent air entrapment.

    Tool venting depth should be 0.02–0.03 mm to prevent burn marks without flash. Clamp force can be estimated at 0.5–0.8 ton/cm² of projected part area, but actual requirements depend on wall thickness, flow length, and packing pressure. Cavity-pressure sensors are recommended when coplanarity or flatness is critical; they permit transfer from velocity control to pressure control before the part becomes over-packed.

    Mold cooling uniformity has a first-order effect on post-mold warpage. Cooling-channel spacing should be no more than 2.5 d from the cavity surface, where d is the channel diameter. Turbulent coolant flow with a Reynolds number above 10,000 is required for uniform heat extraction. Cavity-to-cavity temperature variation greater than ±5°C can produce measurable distortion in flat parts. Post-mold dimensional checks should be made after conditioning at 23°C and 50% relative humidity for 24 h under ISO 291. Shrinkage can continue for up to 48 h after ejection. If annealing is used at 120°C for 2 h to relieve molded-in stress, an additional dimensional movement of up to 0.1% should be expected and compensated in tooling.

    Short-shot studies are used to establish the lower fill limit. Transfer from injection to packing should occur when the end-of-fill pressure begins to rise. Over-packing increases molded-in stress and warpage, whereas under-packing increases sink and dimensional variation. If flash appears at the parting line, packing pressure should be reduced before clamp force is increased. Burn marks typically require improved venting or lower injection velocity; sink marks require longer pack time or reduced melt residence time.

    Electrical, thermal, and chemical exposure data for qualification

    Electrical qualification of PBT-GF grades typically includes dielectric strength under IEC 60243-1 or ASTM D149, volume resistivity under IEC 62631-3-1, and comparative tracking index under IEC 60112. The natural PBT-GF grade is not a flame-retardant formulation; UL 94 classification is generally HB. Applications requiring V-0, V-1, or V-2 ratings must use a flame-retardant Crastin grade and verify the exact thickness in the UL Yellow Card for the final color.

    Thermal parameters include a melting point of 225°C under ISO 11357-3 and heat deflection temperature of 175°C at 1.8 MPa and 215°C at 0.45 MPa under ISO 75-2. Continuous service temperature is not a single material constant; for electrical insulation aging, the relative thermal index under UL 746B or long-term thermal endurance under IEC 60216 must be used from the manufacturer’s current certification file. These values are application-specific and cannot be inferred from short-term HDT alone.

    PBT absorbs less moisture than polyamide, which helps preserve electrical performance in humid environments. However, ester linkages are sensitive to hydrolysis in hot water and steam. Immersion testing under ISO 175 is required when the part contacts aqueous fluids above 60°C. Resistance to mineral oils, greases, and many automotive fluids is generally adequate at operating temperatures below 80°C. Strong acids, strong bases, phenols, ketones, and boiling water are outside the recommended exposure envelope.

    Standard natural PBT has limited ultraviolet resistance; prolonged outdoor exposure can cause surface chalking and embrittlement. The NC010 natural grade is intended for interior or protected applications unless an additional stabilization package is certified for outdoor exposure. Regulatory and food-contact status must be obtained from the supplier for the specific grade and color. Typical PBT compounds are assessed under REACH and RoHS, but the base resin designation alone does not imply food-contact or medical certification.

    When hot-water exposure exceeds 60°C, hydrolytic degradation becomes design-limiting

    Aqueous service conditions require evaluation beyond tensile-specimen comparisons. The ester linkages in PBT undergo chain scission in the presence of water at elevated temperature; the rate increases with temperature, mechanical stress, and pH. Parts exposed to steam sterilisation, engine coolant, or continuous hot-water contact must be tested under application-specific temperature-pressure cycling rather than extrapolated from short-term immersion data alone.

    Published data for this specific configuration is limited for long-term hot-water aging; therefore, qualification programs should include tensile impact retention, molecular weight measurement by intrinsic viscosity or gel permeation chromatography, and dimensional inspection after exposure. For low-pressure aqueous environments below 40°C, the grade can be used without special hydrolysis protection.

    The low-warpage filler package is suited to flat electrical connectors with pin pitch tighter than 2.54 mm, where coplanarity of the molded housing influences terminal insertion force. Molded connectors are evaluated for dimensional tolerance after conditioning, insulation resistance after damp heat under IEC 60068-2-78, and vibration durability under IEC 60068-2-6. The natural color allows custom coloring, but color concentrates can shift shrinkage and reduce impact; validation with the final color masterbatch is required.

    In automotive sensor housings and actuator end caps, the material is selected for stiffness, lower moisture uptake than polyamide, and resistance to mineral oil and grease. Qualification includes thermal cycling under ISO 16750-4 or IEC 60068-2-14, with functional testing after 1,000 h of aging at 85°C and 85% relative humidity. If the environment includes hot-water splash or steam-cleaning, the hydrolysis limits described above must be addressed.

    For appliance housings and support brackets, tooling should use uniform wall thickness to exploit the low-warpage filler. Wall sections from 0.8 mm to 2.5 mm are typical, but abrupt thickness changes create differential cooling and can reintroduce warpage. Weld lines in glass-filled PBT can reduce local failure strain by 30–50% compared with unfilled sections; gate locations should avoid placing weld lines in pressurized or impact-loaded zones.

    Top