| HS Code | 947252 |
| Density | 0.934 g/cm³ |
| Melt Index 190 C 2 16 Kg | 3.5 g/10 min |
| Melting Point | 124 °C |
| Vicat Softening Point | 104 °C |
| Tensile Strength At Yield | 13.8 MPa |
| Tensile Strength At Break | 17.2 MPa |
| Elongation At Break | 800% |
| Flexural Modulus | 427 MPa |
| Hardness Shore D | 50 |
| Environmental Stress Crack Resistance Escr 10 Igepal | >1000 h |
| Brittleness Temperature | < -70 °C |
| Linear Thermal Expansion Coefficient | 1.5E-4 /°C |
As an accredited Braskem ML3400N Rotational Molding Linear Low Density Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Braskem ML3400N rotational molding LLDPE is supplied in 25 kg polyethylene bags on pallets; 1,000 kg bulk bags are also available. |
| Container Loading (20′ FCL) | 20′ FCL: Braskem ML3400N LLDPE rotational molding grade, 25 kg bags, palletized, shrink-wrapped; approximately 20 MT net. |
| Shipping | Braskem ML3400N LLDPE rotational molding resin is supplied in 25 kg PE bags, stacked on pallets, stretch-wrapped, and shipped in clean, dry trucks or containers. Store cool and dry, away from direct sunlight, moisture, and contaminants. Non-hazardous; no special dangerous goods documentation required. Handle carefully to prevent bag damage. |
| Storage | Store Braskem ML3400N Rotational Molding Linear Low Density Polyethylene in a cool, dry, well-ventilated area, away from direct sunlight, heat, ignition sources, strong oxidizers, acids, and alkalis. Keep containers sealed, labeled, and off the floor. Prevent moisture, contamination, and physical damage. Avoid excessive dust and static buildup. Use good housekeeping and appropriate PPE. Follow the SDS and local regulations. |
| Shelf Life | Typically 24 months in original packaging when stored cool, dry, well-ventilated, away from direct sunlight, moisture, and contamination. |
In rotomolded agricultural liquid fertilizer storage, the service environment combines continuous hydrostatic head, contact with nitrogen-containing salt solutions, and long-wave ultraviolet exposure. For vertical cylindrical tanks between 1,000 L and 10,000 L, ML3400N is processed from dry-flowing powder with a nominal density of 0.934 g/cm³ measured per ASTM D792. The melt flow index of 4.0 g/10 min is measured per ASTM D1238 at 190°C and 2.16 kg load. Tank design is normally specified under ASTM D1998 for upright polyethylene storage tanks. When potable water contact is required in dual-use irrigation systems, the finished part must be evaluated under NSF/ANSI 61. Stress crack resistance is assessed by ASTM D1693 or ISO 22088-3. Typical UAN solutions and ammonium polyphosphate suspensions are handled in ambient service between 5°C and 40°C. Chemical resistance is verified by immersion testing per ASTM D543. Flexural modulus is measured by ASTM D790 or ISO 178. The lower modulus of LLDPE relative to homopolymer HDPE permits moderate deformation at boss transitions without cracking.
Dry blending combines ML3400N powder with a carbon black masterbatch at 2.0 wt% to 2.5 wt% for ultraviolet screening. A hindered amine light stabilizer addition of 0.10 wt% to 0.20 wt% is used when tanks are installed in high-sunlight exposure. Primary antioxidant and phosphite secondary antioxidant are retained at 0.05 wt% to 0.10 wt% to preserve melt stability during long oven dwell. Residual stabilizer after regrind exposure is verified by ASTM D3895 oxidative induction time. The powder is pulverized to a nominal 35 mesh (500 µm) particle size. Particle size distribution is checked by dry sieve analysis per ASTM D1921. Apparent density is measured by ASTM D1895. Shot weight is calculated from part surface area and nominal wall thickness plus a 3% closing seam allowance. Oven setpoints in aluminum molds are typically set between 288°C and 316°C. Primary rotation speed is held near 6 rpm and secondary speed near 1.5 rpm to maintain the 4:1 biaxial rotation ratio. Cooling is performed with forced air at 25°C to 30°C and air velocity not exceeding 5 m/s. Water mist is introduced only after mold surface temperature falls below 120°C.
Terminal products include vertical cylindrical storage tanks, conical-bottom agricultural tanks, and field sprayer supply tanks. Fittings and boss inserts are molded-in by placing the insert in the mold cavity before charging. The lower sidewall is intentionally built thicker than the top wall to manage hoop stress. Demolding occurs when the part surface temperature is below 70°C. Residual thermal stress from rapid cooling can lower the effective ESCR. Tanks above 5,000 L are therefore cooled with staged air rather than direct water quench. The operational boundary is that solvent-based pesticide formulations and high-concentration hydrofluoric acid are outside the normal chemical resistance envelope of this configuration.
The regulatory burden for diesel fuel tanks begins with the UN 31A/Y rating when the tank is used as an intermediate bulk container or transport vessel. Rotomolded ML3400N fuel tanks are built with nominal wall thickness not less than 6 mm. The tank must pass hydrostatic pressure, drop impact, leakproofness, and vibration tests. Because hydrocarbon fuel permeates polyethylene slowly, long-term testing is specified under ASTM D2684 or an equivalent permeation protocol. High aromatic content in off-road diesel and biodiesel blends increases swelling. The processing objective is not only burst resistance but also the elimination of pinholes at molded-in fittings. The mold surface temperature must remain uniform around the fill neck insert, which acts as a heat sink and can create a low-density weld line if not preheated with external hot air.
| Test | Standard reference | Production control link |
|---|---|---|
| Leakproofness | 49 CFR 178.703 | Pin-hole detection at molded inserts |
| Hydrostatic pressure | 49 CFR 178.703 | Bottom radius wall uniformity |
| Drop impact | 49 CFR 178.703 | Low-temperature resin toughness |
| Vibration | 49 CFR 178.703 | Baffle and boss fatigue resistance |
For static discharge control, conductive carbon black is compounded into the LLDPE powder at 4 wt% to 8 wt%. Surface resistivity is assessed by ASTM D257. This loading reduces processability and low-temperature impact. The tank wall is usually increased to 8 mm to 10 mm. Internal threads, baffles, and fill neck inserts are molded-in, not post-welded. Conductive carbon black dispersion is checked by optical microscopy on microtomed sections. Poor dispersion creates localized resistivity above 10^9 Ω. This condition can fail the static discharge requirement of local codes and may invalidate the UN certification.
Oven residence time is extended until the internal air temperature measured in the mold reaches 190°C to 205°C. This ensures complete coalescence in the thicker boss areas. The mold is then cooled with forced air. Water spray is delayed until the internal air temperature falls below 100°C. Because conductive carbon black increases melt viscosity, the primary axis speed is lowered to 4 rpm and the secondary axis speed is kept at 1 rpm. This reduces off-axis thinning in the neck region. Finished fuel tanks are dried at 70°C for 2 h before internal inspection with high-intensity white light and pressure-decay testing at 20 kPa.
The terminal article is used for portable diesel transfer tanks, generator day tanks, and UN 31A/Y intermediate bulk containers. Operational boundaries include limited resistance to methanol and strong ketone solvents. Continuous fuel temperature above 50°C is not advised without specific permeation testing. Published data for this specific configuration is limited when tank age exceeds five years. Annual hydrostatic testing at 1.5 times rated head is therefore specified in service maintenance schedules.
Chlorine contact chambers and sodium hypochlorite dosing basins impose a different set of stabilizer demands on rotomolded LLDPE than agricultural duty. Sodium hypochlorite solutions at 5% to 12% available chlorine are commonly stored in natural or white polyethylene tanks at ambient temperature. Chemical resistance is verified by immersion testing per ASTM D543. When treated water is destined for potable use, the tank material and surface must be evaluated under NSF/ANSI 61. The finished part must be free of carbon black surface streaks that can release carbon particles into the stored solution. The tank design is generally rectangular or horizontal cylindrical, with capacities from 200 L to 5,000 L.
This formulation avoids carbon black and conductive fillers. Titanium dioxide is added at 0.5 wt% to 1.0 wt% for opacity. Hindered phenolic antioxidant is used at 0.08 wt% to 0.15 wt%. Phosphite process stabilizer is kept at 0.05 wt% to 0.10 wt%. Metal stearate acid scavengers are minimized because excess zinc stearate reduces environmental stress crack resistance. The powder blend is processed at standard LLDPE oven setpoints. Wall thickness is held at 6 mm to 8 mm for rectangular sidewalls. The cooling cycle must not induce warpage that misaligns flanged connections.
The terminal product includes dosing pump skid tanks, chlorine contact basins, and acid rinse troughs. Fittings are molded from polyethylene or polypropylene and are not solvent-welded. The operational boundary is that concentrated oxidizing acids such as nitric acid above 10% and hot sodium hydroxide above 60°C require chemical resistance testing beyond standard mineral acid exposures.
Wave action and sub-0°C service require the shell to absorb repeated impact without cracking. ML3400N is formed into navigation buoy shells, floating docks, and aquaculture floats. Low-temperature drop-impact performance is measured per ISO 6603-2 on plaques cut from the shell. Outdoor weathering is evaluated under ASTM G154 or ISO 4892-2. The shell is usually produced with a wall thickness of 5 mm to 8 mm. Because the mold is not pressurized, internal air pressure remains atmospheric during the heating stage. Trapped moisture and residual gas can create porosity at the weld line if the powder is not dry-flowing.
The powder is dry-blended with carbon black at 2.0 wt% to 3.0 wt% and a hindered amine light stabilizer at 0.10 wt% to 0.25 wt%. This combination protects against ultraviolet degradation and reduces the development of surface microcracks. The mold is charged with a shot weight calculated for specific surface area. The primary axis speed is set at 5 rpm and the secondary axis speed at 1.2 rpm. The oven setpoint is selected between 280°C and 310°C. The part is cooled slowly to 80°C before water mist contact to avoid warpage in the equatorial seam.
After demolding, closed-cell polyurethane foam of density 32 kg/m³ to 50 kg/m³ is injected into the cavity. The foam provides buoyancy reserve and limits water ingress if the shell is punctured. Terminal buoys are fitted with molded-in chain eyes. The shell must not be produced with internal mold release exceeding 0.10 wt% because excessive release agent can interfere with foam adhesion and paint bonding. This configuration is not used for high-pressure gas containers.
In fork pocket areas and corner blocks, the local wall thickness rises from 6 mm in the deck to 15 mm in reinforcement ribs. This transition creates differential cooling and residual stress. ML3400N is used for hygienic pallets, meat lugs, and freezer aisle dunnage. The rotational molding process produces one-piece double-sided pallets without mechanical fasteners. The pallet is tested under ISO 8611-1 for load-bearing capacity. Impact resistance is verified by ISO 6603-2 puncture impact testing at -20°C. The material must retain impact after prolonged cold storage at -20°C.
For the thick-thin transitions, mold surface temperature must not drop below 70°C before demolding. Forced air cooling starts at 3 m/s. Water mist is introduced only after the mold surface temperature reaches 120°C. Internal air temperature is monitored with a wireless pyrometer; the part is held above 190°C internal air temperature for at least 5 min to collapse bubbles in the thick ribs. Premature water quench causes sink marks in the flat deck and reduces flatness below the tolerance required for automated pallet handling.
The formulation includes a low level of zinc stearate at 0.05 wt% to 0.10 wt% to assist mold release without degrading ESCR. Carbon black is omitted for food-contact pallets unless the end user specifies outdoor use. Terminal products include open-deck pallets, solid deck pallets, and box-style meat lugs. The operational boundary is that racking load above 1,000 kg requires finite element analysis of the molded undercuts and additional wall thickness in the column bosses.
Outdoor playground slides, tunnel segments, and seating shells require bright color retention, low skin abrasion, and impact resistance at ambient outdoor temperatures. The finished component is molded from ML3400N with inorganic pigment masterbatch at 1.0 wt% to 3.0 wt%. Ultraviolet stabilizers are selected from non-blooming hindered amine systems at 0.10 wt% to 0.20 wt%. The material must pass heavy-metal migration limits specified in EN 1176-1 and structural durability clauses of ASTM F1487. Wall thickness is typically 4 mm to 6 mm for large double-wall panels.
The mold is constructed as fabricated sheet metal with polished interior surfaces to maintain gloss and smoothness. Oven setpoints are held in the lower range of 280°C to 295°C to reduce color shift in organic pigments. Rotational speeds are set at 6 rpm primary and 1.5 rpm secondary. Cooling is performed with forced air only; water mist is avoided because rapid cooling causes differential shrink in panels with complex backside ribs. Demolding is performed at 65°C. Terminal products are assembled with through-bolted or molded-in attachment bosses. The operational boundary is that dark colors in high-sunlight regions can develop surface temperature above 60°C and require additional UV stabilizer evaluation.
Electroplating line tanks distinguish themselves by combined exposure to aqueous acids, metal salts, and elevated process temperatures. Rotomolded ML3400N liners are used in rinse tanks, acid etch tanks, and secondary containment basins. Chemical resistance is assessed by ASTM D543 immersion at the specific bath composition and operating temperature. Secondary containment is designed under EPA 40 CFR 264.175 where hazardous waste is present. The tank wall is generally 8 mm to 12 mm for free-standing rectangular vessels. The liner is not intended for unlined steel tank replacement when the operating temperature exceeds 60°C.
Internal air release packages are required to prevent bubble entrapment in large flat sidewalls. Zinc stearate is added at 0.05 wt% to 0.10 wt%. Higher zinc stearate loadings reduce bubble defects but lower environmental stress crack resistance and can interfere with adhesion of surface coatings. Talc nucleating agents are avoided in acid service because exposed talc particles can increase surface roughness and create localized attack sites. The powder is processed with oven setpoints between 288°C and 315°C. The primary axis speed is reduced to 4 rpm for deep vertical tanks to improve wall distribution in the corners.
The terminal product is a one-piece seamless liner with molded-in flange edges and overflow weirs. Wall thickness is verified by ultrasonic thickness gauge in the lower corners and at the flange. Dimensional inspection includes corner radius measurement. The tank must be free of visible pinholes when tested with high-intensity light and low-pressure air at 15 kPa. The operational boundary is that aromatic solvents and strong oxidizing acids are not recommended. For chromium etching baths above 40°C, resin-specific chemical compatibility must be confirmed before fabrication.
Competitive Braskem ML3400N Rotational Molding Linear Low Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Braskem ML3400N is a linear low-density polyethylene intended for single-layer rotational molding of seamless hollow articles. The grade is identified by a nominal density of 0.940 g/cm³ determined in accordance with ASTM D1505, and a melt mass-flow rate of 4.0 g/10 min under 2.16 kg at 190°C in accordance with ASTM D1238 / ISO 1133-1:2022. The product is supplied as a powder with a controlled particle size distribution suited to biaxial rotational molding equipment. The polymer architecture is based on an ethylene/alpha-olefin copolymer with short-chain branching that reduces crystalline density relative to high-pressure LDPE while retaining sufficient interlaminar chain entanglement to improve resistance to slow crack growth in service.
In the rotational molding conversion sequence, the powdered charge is placed in a closed mold, heated under biaxial rotation, sintered at the mold surface, and cooled under controlled air or water-mist conditions. The grade is used for agricultural water storage tanks, chemical dosing containers, material handling bins, recreational components, and industrial covers where a balance of stiffness, impact strength, and environmental stress crack resistance is required. The product is not intended for pressure-pipe extrusion, film blowing, or injection molding without independent rheological and oxidative stability evaluation.
The primary structural distinction is crystallinity control. Conventional rotational molding HDPE grades are typically supplied in the 0.945–0.955 g/cm³ density range. At equivalent wall thickness, those grades develop higher flexural modulus but can exhibit reduced resistance to brittle crack propagation at stress concentrations such as molded-in inserts, sharp corner radii, or weld-line regions generated by uneven powder coalescence. ML3400N, at 0.940 g/cm³, places the polymer in the intermediate-density LLDPE roto-grade range. The lower crystalline fraction and higher tie-molecule population contribute to a measurable shift in environmental stress cracking resistance under ASTM D1693. However, direct comparison with a specific HDPE grade should not be inferred from nominal density alone. ASTM D1693 F50 data are strongly dependent on specimen thickness, notch depth, mold cooling rate, and conditioning temperature. Laboratories evaluating alternative materials should compression mold both candidates in the same tooling and test them under identical conditions.
Compared with lower-density LLDPE rotomolding grades near 0.930–0.935 g/cm³, ML3400N shifts the property envelope toward higher flexural modulus and greater resistance to distortion under hydrostatic load. The trade-off is a reduction in low-temperature ductility and a slightly narrower processing window at low peak internal air temperature. The melt flow index of 4.0 g/10 min supports adequate spiral flow into complex mold geometries while retaining higher zero-shear viscosity than fractional-melt grades. On multi-cavity shuttle machines with biaxial rotation ratios near 4:1, this melt flow range provides consistent wall thickness distribution in rectangular tanks with recessed handles and threaded bosses.
Under lot acceptance testing, the following nominal values are applied to release the product for rotational molding. The values are not intended as guaranteed specification limits; actual lot-specific certificates of analysis should govern acceptance decisions.
| Property | Standard | Nominal value |
|---|---|---|
| Density | ASTM D1505 | 0.940 g/cm³ |
| Melt mass-flow rate | ASTM D1238 | 4.0 g/10 min |
| Tensile strength at yield | ASTM D638 Type IV | 17 MPa |
| Elongation at break | ASTM D638 | >800% |
| Flexural modulus, 1% secant | ASTM D790 | 700 MPa |
| Environmental stress crack resistance, F50 | ASTM D1693 Condition A | >1,000 h |
| Vicat softening temperature | ASTM D1525 Rate B | 117°C |
| Brittleness temperature | ASTM D746 | <-75°C |
The tensile and flexural values are obtained on compression-molded plaques, not on rotationally molded parts. Because rotomolding produces a gradient in crystalline morphology through the wall thickness, part-level mechanical properties may differ from plaque data. Wall thickness, cooling rate, mold surface finish, and pigment loading alter residual stress and impact response. Validation on production-scale tooling is required before substituting ML3400N into an existing HDPE or lower-density LLDPE part number.
ML3400N is supplied as a rotomolding powder; pulverization is not required for incoming material unless pelletized packaging formats are specified. The powder should exhibit a dry-flow time of approximately 28–32 s/100 g when measured according to ASTM D1895 Method A. Bulk density is typically maintained in the range of 0.35–0.40 g/cm³. Screen analysis normally shows a high proportion passing a 35 mesh screen, with limited fines below 200 mesh. Excess fines can reduce dry flow and lead to uneven charge distribution in narrow mold cavities. Excess coarse particles can remain unmelted at the inner wall if the peak internal air temperature is too low, producing pinholes or poor inner-surface uniformity.
On production shuttle-style rotational molding machines, the mold is rotated at primary and secondary speeds that produce a typical ratio of 4:1. Oven setpoints are commonly held between 280°C and 300°C for wall thicknesses up to 6.0 mm. The controlling variable is peak internal air temperature measured by vent thermocouples. For ML3400N, peak internal air temperature is typically maintained between 195°C and 205°C. If the peak internal air temperature remains below 190°C, sintering may be incomplete and the inner surface may retain visible powder grain boundaries. If the peak internal air temperature exceeds 220°C, oxidative degradation accelerates, producing yellowing, embrittlement, and surface pinholes. The acceptable temperature window is therefore narrow by rotational molding standards, and cycle development should include polymer melt temperature mapping rather than oven timer adjustment alone.
Cooling must also be controlled. Forced-air cooling should reduce the mold surface temperature to approximately 90°C before water mist or closed-loop water spray is introduced. Removing the part above 70°C can cause warpage, especially in flat panel sections and large-diameter bases. Slow cooling through the crystallization range improves impact strength but increases cycle time; rapid cooling increases productivity but may raise molded-in stress. Parts with threaded inserts or metal bosses should be cooled more slowly to prevent insert separation. Production-scale experience indicates that inadequate cooling below the crystallization range is a more common source of field returns than oven temperature deviation.
Environmental stress crack resistance under ASTM D1693 is a key selection criterion for tanks exposed to detergents, agricultural adjuvants, or quaternary ammonium disinfectants. The short-chain branching in ML3400N reduces crack propagation at notched surfaces relative to higher-density rotomolding grades. However, ESCR is not an intrinsic material constant. Molded-in notch sensitivity, sharp internal corners, metal insert geometry, and high residual stress from rapid cooling can reduce service life even when the resin F50 value exceeds 1,000 h. For chemical contact applications, the specific chemical formulation, concentration, temperature, and stress state must be evaluated by immersion testing rather than inferred from generic polyethylene compatibility tables.
Oxidative stability is process- and service-dependent. The resin requires a heat stabilization package for rotomolding because the powder is exposed to air at high temperature during the oven cycle. Oxidation induction time measured by differential scanning calorimetry can be used to compare formulations, but published data for ML3400N under all pigmented and regrind conditions is limited. Unpigmented parts used outdoors will degrade under ultraviolet exposure. For outdoor service, a carbon black loading of 2.0–3.0 wt% or an appropriate hindered amine light stabilizer package is required. Without UV stabilization, surface chalking and embrittlement can occur within 12–24 months in high-UV environments. The exact failure time depends on wall thickness, part orientation, and operating temperature.
When regrind is incorporated into the rotomolding charge, the particle size distribution broadens and dry-flow time increases. Ground moldings retain the stabilizer history of the original part but also carry accumulated heat history. Regrind levels above 20 wt% should be validated by checking oven-cycle performance, inner-surface smoothness, and impact resistance on production-scale test parts. Regrind should be free of foreign polymer residues, metal shavings, and moisture condensation. Storage under high relative humidity can deposit free water on the powder, which may create steam pinholes during the early stages of oven heating if the mold is charged cold.
In rotational molding of agricultural water storage tanks, the wall thickness is typically specified between 6.0 mm and 8.0 mm to accommodate hydrostatic stress and long-term outdoor exposure. The mold is charged with enough powder to achieve the target wall thickness, rotated at the prescribed primary and secondary speeds, and heated until the peak internal air temperature reaches the 195–205°C range. After cooling and demolding, the part is inspected for uniform wall thickness, internal surface porosity, and insert integrity. Field performance is then governed by chemical exposure, UV load, and mechanical stress concentration at mounting points and drain fittings.