| HS Code | 161701 |
| Polymer Type | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | Butene-1 |
| Melt Index | 0.5 g/10 min at 190°C/2.16 kg |
| Density | 0.918 g/cm³ |
| Melting Point | 121 °C |
| Vicat Softening Point | 95 °C |
| Crystallization Temperature | 100 °C |
| Tensile Strength At Yield Md | 11 MPa |
| Tensile Strength At Yield Td | 10 MPa |
| Tensile Strength At Break Md | 28 MPa |
| Tensile Strength At Break Td | 24 MPa |
| Elongation At Break Md | 700 % |
| Elongation At Break Td | 800 % |
| Elmendorf Tear Strength Md | 250 g |
| Elmendorf Tear Strength Td | 400 g |
| Dart Impact Strength | 200 g |
| Haze | 10 % |
| Gloss 45 | 60 % |
| Coefficient Of Friction | 0.20 |
As an accredited Braskem LL5405S Blown Film Extrusion Linear Low Density Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Braskem LL5405S Blown Film Extrusion LLDPE is packaged in 25 kg polyethylene bags, palletized and stretch-wrapped. |
| Container Loading (20′ FCL) | Braskem LL5405S Blown Film Extrusion Linear Low Density Polyethylene in 20′ FCL: dry container, palletized 25 kg bags, secured, ambient. |
| Shipping | Typically, Braskem LL5405S is shipped as non-hazardous LLDPE pellets in moisture-barrier bags, octabins, or bulk trucks/railcars. Store in a cool, dry, clean area away from direct sunlight, heat, and contaminants. No special DOT/IMDG/IATA hazard classification applies; maintain packaging integrity to prevent spillage and moisture pickup during transport. |
| Storage | Store Braskem LL5405S LLDPE blown-film resin in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, and open flames. Keep original bags or containers tightly closed on pallets, protected from moisture, dust, and contamination. Avoid prolonged high temperatures and incompatible oxidizers. Use first-in, first-out stock rotation. Follow supplier SDS and local regulations for safe handling and housekeeping. |
| Shelf Life | Shelf life typically 12 months in unopened original packaging, stored cool, dry, away from direct sunlight; verify with supplier. |
Braskem LL5405S is a blown film extrusion grade linear low density polyethylene with a nominal melt index of 1.0 g/10 min when measured under ASTM D1238 at 190°C and 2.16 kg and a nominal density of 0.918 g/cm³ under ASTM D792. In heavy-duty shipping sacks, the resin is processed at 100 wt% or in dry blends containing 10 wt% to 20 wt% low-density polyethylene. The LDPE fraction reduces melt pressure and stabilises the bubble at low film thickness. On a 70 mm single-screw extruder with 28:1 L/D and a 100 mm blown film die, the die gap is set between 1.6 mm and 2.0 mm. The blow-up ratio is held at 2.2:1 to 2.8:1. Frost line height is maintained between 450 mm and 650 mm for a 120 µm monolayer sack. Melt temperature at the die is controlled between 195°C and 220°C to suppress oxidative gel formation. Edge trim regrind is used up to 20 wt% in the core layer of a three-layer sack because gel count increases beyond this level. Terminal sacks for polymer granules, mineral fillers, and fertiliser are tested for dart drop impact under ASTM D1709 Method B. Tensile properties are recorded under ASTM D882. Elmendorf tear propagation is measured under ASTM D1922. Where the sack is used as UN certified packaging, the performance follows drop and stacking tests described in Chapter 6.5 of the UN Model Regulations. The converter must run batch-to-batch melt index checks because variation above ±0.1 g/10 min alters bubble stability at 120 µm and shifts the frost line into a lower neck region that reduces transverse tear resistance.
| Parameter | Heavy-duty sack film 120 µm | Frozen food sealant layer 50 µm | Can liner 25 µm |
|---|---|---|---|
| Die gap | 1.6–2.0 mm | 1.4–1.8 mm | 1.0–1.4 mm |
| Blow-up ratio | 2.2:1–2.8:1 | 2.0:1–2.2:1 | 2.5:1–3.0:1 |
| Melt temperature | 195–220°C | 200–215°C | 200–225°C |
| Frost line height | 450–650 mm | 300–450 mm | <400 mm |
In frozen food packaging, LL5405S is placed into the sealant layer of a three-layer or five-layer polyethylene blown film. The sealant layer typically occupies 20% to 30% of the total gauge. At total film thickness of 50 µm, the sealant layer is 10 µm to 15 µm. The film is produced on a 250 mm multi-layer die with 1.8 mm die gap and 2.0:1 blow-up ratio. Melt temperature at the sealant extruder is kept at 200°C to 215°C because a higher sealant-layer melt temperature narrows the hot tack window and promotes seal-surface irregularity. The slip additive concentration in the sealant layer is held below 1,000 ppm because migration above this level can reduce seal strength under ASTM F88 by more than 10%. The terminal bags are used for IQF vegetables, seafood, and portion-controlled frozen prepared food. Heat seal characteristics are evaluated under ASTM F2029. For butene LLDPE of 0.918 g/cm³ density, the seal initiation temperature is generally observed in the 95°C to 105°C band when jaw pressure is 2.7 bar and dwell time is 0.5 s. Hot tack is measured under ASTM F1921. Seal strength is measured after 24 h conditioning under ASTM F88. Compliance for food contact requires verification under EU 10/2011 and FDA 21 CFR 177.1520. The overall migration limit is 10 mg/dm² under EU 10/2011 for plastic materials in contact with food. Converters must confirm that antioxidants or slip additives in the final formulation do not exceed the specific migration limits of Annex I of that regulation. The operational boundary is the seal bar temperature. Below 90°C, seal strength is not sufficient for frozen distribution. Above 115°C, the film can shrink at the seal jaw and produce pleats that compromise pack integrity.
Collation shrink films containing LL5405S are formulated in a narrow blending window of 70 wt% to 80 wt% LLDPE and 20 wt% to 30 wt% LDPE. The LDPE component is not added for cost control only. It increases machine-direction shrink tension and accelerates bubble cooling. A monolayer or three-layer line with a 1.2 mm die gap and 3.0:1 blow-up ratio is used. The high stalk is maintained at a frost line height of 350 mm to 500 mm. Film thickness is 40 µm to 70 µm. Under ASTM D2732, unrestrained linear thermal shrinkage in the machine direction is typically in the 60% to 75% range at 160°C, while transverse direction shrinkage remains below 15%. Shrink force is checked under ISO 14616. The terminal product is bottle multipack collation and printed film overwrap for cans. A processing boundary exists at LDPE addition above 30 wt%. The bubble enters a less stable corridor because the high-molecular-weight LDPE fraction increases melt strength but reduces the dart drop of the final shrink film. Below 20 wt% LDPE, the machine-direction shrink tension is insufficient to hold bottle groups under transit vibration. The converter adjusts the collapsing frame angle and uses a low-pressure dual-lip air ring to avoid gauge variation above ±8% because shrink force is proportional to local gauge. Batch-to-batch LDPE melt index changes above 0.4 g/10 min shift the required frost line height and can produce irregular shrink windows.
| Downstream application | Standard designation | Test or compliance parameter |
|---|---|---|
| Heavy-duty shipping sacks | ASTM D1709, ASTM D882, ASTM D1922 | Dart impact, tensile, Elmendorf tear |
| Frozen food packaging | ASTM F2029, ASTM F1921, EU 10/2011 | Heat seal, hot tack, overall migration |
| Agricultural films | EN 13206, ASTM D1709 | Weathered tensile and impact |
| Collation shrink | ASTM D2732, ISO 14616 | Unrestrained linear shrinkage, shrink force |
| Can liners | ASTM D1709, ASTM D1922, ASTM D882 | Dart impact, Elmendorf tear, tensile |
| Lamination base films | ASTM D2578, ASTM F904 | Wetting tension, bond strength |
For agricultural low tunnels and silage cover film, LL5405S is used in monolayer and three-layer structures at total thickness between 50 µm and 150 µm. The film is blown through a 200 mm die with 2.0 mm die gap at 2.4:1 blow-up ratio. A frost line height of 500 mm to 700 mm is maintained. The extruder barrel profile is set from 180°C at the feed throat to 210°C at the adapter. UV stabiliser masterbatch is let down at 4 wt% to 6 wt% in the core layer, and anti-fog additive masterbatch is introduced at 2 wt% to 3 wt% in the inside skin layer only. For three-layer film, the layer ratio is 30% skin / 40% core / 30% skin. Tensile strength is tested under ASTM D882. Impact resistance is verified under ASTM D1709 Method B. The finished film is used as low-tunnel cover, silage clamp cover, and overwintering film for nursery stock. Compliance is linked to EN 13206 for covering films used in agriculture and horticulture. The standard requires minimum tensile and impact properties after weathering exposure. The film must be stored in a temperature-controlled warehouse below 35°C because uncontrolled UV masterbatch dispersion can produce local thinning when regrind is reused above 10 wt%. The major operational boundary is film gauge uniformity. A variation greater than ±10% across the web reduces the weathering life of thin sections and creates premature failure under wind load on low-tunnel structures.
Monolayer can liners are produced at 20 µm to 35 µm from LL5405S as a 100 wt% resin or as a blend with 10 wt% to 30 wt% HDPE. The HDPE fraction increases the secant modulus for easy bag opening but reduces dart drop impact. On a 60 mm extruder with 24:1 L/D and 120 mm die, the die gap is set at 1.0 mm to 1.4 mm. The blow-up ratio is 2.5:1 to 3.0:1. Melt temperature is held at 200°C to 225°C. At 20 µm, bubble stability is the primary bottleneck. The frost line height is kept below 400 mm to prevent the bubble from wandering. Above take-off speeds of 35 m/min, draw resonance may appear as alternating thick and thin bands. Terminal products are refuse can liners and retail produce bags. Film is tested for dart drop under ASTM D1709 Method A. At 25 µm, dart drop values in the 90 g to 160 g range are typical for this density class. The lower limit is governed by the film gauge. Elmendorf tear is measured under ASTM D1922. Machine-direction tear is usually lower than transverse direction tear because molecular orientation is higher in the machine direction. The converter must monitor ambient air temperature. Below 15°C, the film cooling rate increases and film stiffness increases, which can generate poor bag opening and static cling. Blending above 30 wt% HDPE is not recommended because the dart drop falls below the level required for heavy refuse load retention.
Lamination base film made from LL5405S is blown at 15 µm to 25 µm for subsequent adhesive lamination to biaxially oriented polyester or biaxially oriented polypropylene. The film is corona treated in-line to a wetting tension of 38 mN/m to 42 mN/m measured by ASTM D2578. The die gap is set at 0.8 mm to 1.2 mm. The blow-up ratio is held at 2.0:1 to 2.3:1. Cooling air is directed through a dual-lip air ring at low velocity to limit haze. The extruder melt temperature is kept at 195°C to 210°C. At die gaps below 1.2 mm, the thin melt curtain becomes sensitive to changes in die lip cleanliness and melt temperature variation. The terminal laminate is used in wrap-around labels, snack packaging, and coffee pouches. For food contact, the final laminate must comply with EU 10/2011 and FDA 21 CFR 177.1520. The converter runs the lamination substrate at 0.3% to 0.5% slip additive by weight only when the downstream converter confirms that the slip additive has no adverse effect on lamination bond strength after 24 h curing. The lamination bond strength is checked under ASTM F904 using a heat-seal bond tester. Surface treatment must be re-verified before winding because corona decay can reduce wetting tension by 4 mN/m to 6 mN/m within 72 h on untreated film. Film is wound with taper tension of 12–15 N/100 mm width to prevent blocking. The primary failure mode on the laminator is poor wet-out when the wetting tension drops below 38 mN/m, causing the adhesive to de-wet on the LLDPE surface and reducing bond strength below the acceptable 60 g/25 mm seal-strength threshold used in flexible packaging quality control.
Competitive Braskem LL5405S Blown Film Extrusion Linear Low Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Braskem LL5405S is a butene-based linear low density polyethylene produced by the low-pressure gas-phase polymerization process. The resin is supplied in pellet form and is intended for blown film extrusion. Nominal density is 0.916 g/cm³ when measured by ASTM D792 or ISO 1183-1, and melt flow rate is 1.0 g/10 min at 190°C under 2.16 kg load when tested by ASTM D1238 or ISO 1133-1. Butene comonomer introduces short-chain branching that lowers crystalline lamellae thickness relative to high-pressure LDPE, increasing elongation at break and puncture resistance while reducing melt strength. The Ziegler-Natta molecular architecture produces a broader melting range and higher seal initiation temperature than metallocene-catalyzed hexene LLDPE of similar density. The pellet stabilizer system includes a hindered phenolic primary antioxidant and a phosphite secondary antioxidant, with typical ash content below 0.05 wt%. Published data for this specific configuration is limited for blends containing post-consumer reclaim; processors should monitor filter pressure rise and gel formation when adding recycled polyethylene.
On a 60 mm grooved-feed single-screw extruder with L/D 30:1 and a 200 mm blown film die, LL5405S is typically started with a barrel profile ascending from 170°C at the feed section to 205°C in the metering section, with adapter and die zones set at 210°C. Melt temperature at the extruder discharge is maintained below 230°C. Residence times above 30 min at melt temperatures above 240°C increase yellowness index and gel formation because of antioxidant depletion. The die gap is typically set between 1.8 mm and 2.4 mm, which is wider than the 0.8–1.2 mm gap commonly used for high-pressure LDPE. This wider gap reduces die wall shear stress and decreases sharkskin melt fracture at equivalent throughput.
Butene LLDPE has lower melt strength than LDPE; therefore, a dual-lip air ring and internal bubble cooling are preferred to stabilize the bubble. A blow-up ratio between 2.0:1 and 2.8:1 balances MD and TD tear strength. Below 2.0:1, TD tear declines; above 2.8:1, bubble flutter and gauge variation increase. Frost line height is maintained between 4 and 8 die diameters. Lower frost lines improve impact strength, while higher frost lines reduce haze but can lower dart drop because of slower stress relaxation. At throughputs above 180 kg/h on a 75 mm extruder with die diameter 250 mm, the limiting factor is often bubble stability rather than drive amperage; increasing die gap from 1.2 mm to 2.0 mm and lowering melt temperature from 225°C to 205°C has been reported to improve gauge uniformity from ±8% to ±4% in commercial line trials.
Pellets stored under dry indoor conditions do not require pre-drying. If the resin is exposed to relative humidity above 60% and subsequently cooled, surface moisture can produce bubble defects. Drying in a desiccant hot-air system at 65°C for 4 h is sufficient to remove surface moisture. Avoid direct contact with copper alloys, oxidizing acids, and residues from PVC processing because these materials can accelerate polyolefin chain scission and generate gel defects.
Film property ranges for 25 µm monolayer film produced at 2.5:1 blow-up ratio are summarized below. Values are direction-dependent and are influenced by die gap, frost line height, and cooling air temperature. Published data for this specific configuration is limited; the ranges below represent typical results from a 60 mm line with die diameter 200 mm and should be confirmed on the production line.
| Property | Test Method | Unit | Typical Range |
|---|---|---|---|
| Tensile strength at break, MD | ASTM D882 | MPa | 28–38 |
| Tensile strength at break, TD | ASTM D882 | MPa | 22–32 |
| Elongation at break, MD | ASTM D882 | % | 650–850 |
| Elongation at break, TD | ASTM D882 | % | 750–950 |
| Elmendorf tear resistance, MD | ASTM D1922 | gf | 200–400 |
| Elmendorf tear resistance, TD | ASTM D1922 | gf | 350–550 |
| Dart drop impact, Method A | ASTM D1709A | g | 80–130 |
| Haze | ASTM D1003 | % | 8–15 |
| Gloss at 60° | ASTM D2457 | GU | 50–70 |
These mechanical and optical values position LL5405S in heavy-duty shipping sacks, industrial liners, agricultural film, and coextruded sealant webs. In stretch film, the resin is commonly blended with metallocene hexene LLDPE at 20–40 wt% to increase puncture and MD elongation while retaining cling performance. The grade is not intended for high-clarity retail packaging unless it is used as a core layer or blended with an LDPE skin; haze and gloss values reflect the surface roughness and crystalline texture characteristic of butene LLDPE. The standard pellet does not contain high levels of slip or antiblock. Film-to-film coefficient of friction without masterbatch addition generally remains above 0.4 when measured by ASTM D1894, so converters usually add 1–2 wt% of a compatible slip/antiblock masterbatch for high-speed converting.
In coextruded structures, LL5405S is used as a toughness layer in high-strength films. A three-layer A/B/A structure with an LL5405S core and LDPE skins can achieve a dart drop value 10–20% higher than a monolayer LDPE at the same total thickness, while retaining surface optics and sealing characteristics of the skins. The core layer melt temperature is maintained at 210°C to match the viscosity of typical LDPE skins. Layer ratio variation beyond ±2% can cause curl because of differing shrinkage between LLDPE and LDPE. At thicknesses below 15 µm, gauge uniformity of LL5405S becomes the limiting factor for dart drop; a die gap above 1.8 mm and internal bubble cooling are required to hold film thickness tolerance at ±5%.
Relative to high-pressure LDPE of similar melt flow rate, LL5405S exhibits tensile strength at break values that are approximately 30–50% higher and elongation at break values that are 10–25% higher when tested by ASTM D882. Dart drop impact for 25 µm butene LLDPE film typically falls in the range 80–130 g, while a 0.923 g/cm³ LDPE film of the same thickness often falls below 60 g. However, high-pressure LDPE retains higher melt strength, more pronounced extension thickening, and better bubble stability at high blow-up ratios, which is why LL5405S is usually processed with a wider die gap and higher frost line than LDPE.
Compared with hexene or octene LLDPE grades, LL5405S exhibits lower dart drop and Elmendorf tear because butene short-chain branches are less efficient at forming tie molecules and delocalizing stress at crack tips. A 25 µm hexene LLDPE film can show dart drop values from 150 g to 220 g under equivalent conditions, and machine-direction Elmendorf tear is often 30–50% higher. The effect is more pronounced at temperatures below -30°C; therefore, freezer packaging and cold-chain transport sacks generally use hexene or octene LLDPE. The sealing initiation temperature of LL5405S, evaluated by ASTM F88, is typically 10–15°C higher than that of metallocene hexene LLDPE. Differential scanning calorimetry at 10°C/min generally places the peak melting temperature in the range 120–126°C and the crystallization temperature in the range 104–110°C.
Sealant layers based on LL5405S are used in vertical form-fill-seal packaging at line speeds above 60 packages/min. The hot-tack strength must be matched to the jaw geometry and dwell time; insufficient hot tack causes seal creep during product drop. When LL5405S is blended with up to 20 wt% LDPE, melt strength increases and seal lock-up is reduced, but additions above 20 wt% lower dart drop and Elmendorf tear. Corona treatment is generally required before printing or lamination. A target surface energy of 38–42 mN/m is adequate for solvent-based inks and polyurethane adhesives; treatment above 46 mN/m may induce film wrinkling because of elevated local surface temperature. The film is incompatible with aromatic hydrocarbon solvents in high concentration, and prolonged contact with toluene or xylene at temperatures above 40°C can swell and distort the film.
During slitting, edge trim must be removed with a vacuum system because butene LLDPE has higher elongation than LDPE and generates stretchy trim that can wrap idler rolls. Winding tension is normally set between 10 N/m and 20 N/m per micrometer of film thickness to avoid blocking. At tension above 25 N/m/µm, core crush and gauge banding are observed on rewind stands. These converting boundaries are most visible on films thinner than 20 µm.
Compliance is determined by the finished package, not the resin pellet alone. The base olefin polymer may be evaluated under FDA 21 CFR 177.1520 for food contact, but the overall article must also meet additive migration limits and end-use conditions. The following matrix summarizes references that apply to packages made from LL5405S; converters are responsible for verifying the specific film structure, masterbatch additions, and processing residuals against the applicable regional requirements.
| Scope | Reference | Boundary |
|---|---|---|
| US food contact | FDA 21 CFR 177.1520 | Olefin polymer base resin; end-use condition and additive confirmation required for the final article. |
| EU food contact | EU Regulation 10/2011 | Overall migration below 10 mg/dm² for general food contact; specific migration limits depend on additive package. |
| Packaging heavy metals | EU Directive 94/62/EC | Sum of lead, cadmium, mercury, and hexavalent chromium below 100 ppm by weight in packaging. |
| REACH | REACH Regulation (EC) No 1907/2006 | Polymer itself exempt as a substance under Article 2(9); monomers and additives must be registered. |
Pellets should be stored in dry, clean areas at temperatures below 40°C and protected from direct sunlight. At temperatures above 40°C, pellet caking can occur in stacked supersacks, especially if fine material is present. Silo extraction with mass-flow hoppers having a half angle below 60° avoids bridging. The product should not be processed in equipment previously used for PVC without purging because acidic degradation residues can accelerate chain scission and produce black specks. Blending with polypropylene at levels above 5 wt% is not recommended because the immiscible domains reduce tear resistance and can delaminate in coextruded structures.