| HS Code | 306991 |
| Melt Flow Rate 190 C 2 16 Kg | 2.1 g/10 min |
| Density | 0.918 g/cm³ |
| Melting Point | 120 °C |
| Vicat Softening Point | 94 °C |
| Tensile Strength At Yield | 10 MPa |
| Tensile Strength At Break | 20 MPa |
| Elongation At Break | 700% |
| Dart Impact | 80 g |
| Elmendorf Tear Strength Md | 150 g |
| Elmendorf Tear Strength Td | 300 g |
| Haze | 12% |
| Gloss 45 | 50 |
| Coefficient Of Friction | 0.2 |
| Flexural Modulus | 240 MPa |
As an accredited Braskem LL 118/21 LLDPE Blown Film Extrusion Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaged in 25 kg moisture-resistant polyethylene bags, palletized; each pallet contains 1,000 kg of Braskem LL 118/21 LLDPE resin. |
| Container Loading (20′ FCL) | 20′ FCL loaded with palletized Braskem LL 118/21 LLDPE Blown Film Extrusion Polyethylene bags, shrink-wrapped and secured for ocean shipment. |
| Shipping | Braskem LL 118/21 LLDPE is a non-hazardous polyethylene resin in pellet form. Ship in sealed 25 kg bags or octabins, palletized and stretch-wrapped. Transport in clean, dry, covered containers at ambient temperature, avoiding moisture, direct sunlight, heat, and contamination. Not regulated for transport. |
| Storage | Store in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, flames, and strong oxidizers. Keep original packaging closed to prevent moisture, dust, and contamination. Maintain ambient temperature, avoid prolonged UV exposure, and stack pallets securely to prevent bag damage. Protect from physical damage and follow first-in, first-out inventory practices. |
| Shelf Life | Stable under normal storage; recommended shelf life 12 months when stored cool, dry, sealed, and away from direct sunlight. |
Converters targeting puncture resistance at -20°C in frozen vegetable and seafood packaging evaluate LL 118/21 as the skin layer of a three-layer symmetrical blown film structure. The resin carries a published density of 0.918 g/cm³ under ISO 1183-1 and a melt flow rate of 2.1 g/10 min at 190°C/2.16 kg under ISO 1133-1:2022. In a typical skin-core-skin formulation, the core contains 25 wt% LDPE with a melt flow rate close to 0.3 g/10 min to stabilize the bubble, while each skin contains 70 wt% LL 118/21 and 5 wt% HDPE to control blocking. Slip and antiblock masterbatches are added at 0.4 wt% to 0.8 wt% total, producing a kinetic coefficient of friction below 0.25 measured by ISO 8295. Extrusion on a 65 mm grooved-feed extruder with L/D 30:1 is carried out with barrel set points from 175°C to 205°C, a die temperature of 195°C, and a die gap of 1.8 mm. The blow-up ratio is held at 2.0:1 to 2.4:1 and the frost line height at 300 mm to 450 mm from the die face. Final film thickness for vegetable bags is 35 µm to 45 µm. The structure meets FDA 21 CFR 177.1520 paragraph (c) 2.2 for aqueous and fatty foods under refrigerated and frozen conditions. European compliance is assessed under Regulation (EU) No 10/2011 with an overall migration limit of 10 mg/dm² by EN 1186-1. Low-temperature dart impact is characterized by ASTM D1709-16a method A. Direct comparisons across formulations require film thickness normalization because dart impact is thickness-dependent under this method. Increasing HDPE in the skin above 10 wt% raises secant modulus but degrades MD Elmendorf tear measured by ASTM D1922-15.
Pelletized mineral fillers and granular chemicals packed in 25 kg heavy-duty sacks impose concentrated impact loads at bag drop and edge tear during filling line handling. A coextruded three-layer sack film uses 60 wt% LL 118/21, 25 wt% HMWHDPE with density 0.944 g/cm³ to 0.950 g/cm³, and 15 wt% edge trim recyclate from the same line. The film is extruded on a 80 mm grooved-feed extruder with L/D 26:1, using a 2.0 mm die gap, a melt temperature of 195°C to 205°C, and a blow-up ratio of 1.8:1 to 2.2:1. The frost line is positioned at 500 mm to 700 mm above the die to orient the film and increase MD tear resistance. Total film thickness is 80 µm to 100 µm. Drop resistance is verified by ISO 7965-2 with filled sacks dropped from 1.2 m on face, edge, and butt positions. Dart impact is measured by ASTM D1709-16a method B because the thickness exceeds 50 µm. Tear resistance is reported as ASTM D1922-15 Elmendorf; minimizing HMWHDPE content above 30 wt% is critical because MD tear declines sharply when the HDPE phase forms a continuous load-bearing network. A 3 wt% calcium carbonate masterbatch is included to lower surface slip during filling, but loadings above 5 wt% reduce the molten film bubble stability and create gel-like agglomerates if dispersion is poor. The finished film is not intended for food contact; REACH information for imported sacks is maintained under Article 33 for substances of very high concern.
Agricultural bale wraps for fermented forage require puncture resistance during high-density baling and oxygen transmission below 8,000 cm³/(m²·d·atm) to limit aerobic spoilage by yeasts and molds. LL 118/21 is used in the outer skins of a five-layer blown coextrusion at 65 wt% to 75 wt% in each skin, combined with 20 wt% LDPE and 5 wt% metallocene LLDPE to raise hot tack at the seal. The barrier core is an EVOH grade with 32 mol% ethylene at 5 wt% of total structure, positioned between two tie layers. PIB tackifier is added at 1 wt% to the outer skin only, migrating to the surface to develop cling. The UV stabilization package consists of a hindered amine light stabilizer at 0.2 wt% and a benzotriazole UV absorber at 0.1 wt% based on total film weight. Extrusion uses a 1.6 mm die gap, a blow-up ratio of 2.5:1 to 3.0:1, and a melt temperature of 190°C to 200°C. Film thickness is 25 µm to 30 µm. Oxygen transmission measured by ASTM D3985-17 at 23°C and 0% RH remains below 5,000 cm³/(m²·d·atm) for the multilayer structure. Puncture resistance is characterized by ASTM D5748-18. Outdoor exposure trials in silage baling operations show that failure initiates at edge folds when the tackified skin is reversed during winding, which is an operational boundary rather than a resin limitation.
In laminated stand-up pouches for dry foods and wipes, LL 118/21 functions as the sealant ply because its butene comonomer distribution yields a heat seal initiation plateau between 105°C and 150°C and stable hot tack at line speeds above 40 m/min. The sealant film is coextruded as a monolayer or as the sealant skin of a two-layer structure with 90 wt% LL 118/21 and 10 wt% metallocene LLDPE having density 0.912 g/cm³. The die gap is 1.4 mm, the blow-up ratio is 2.2:1, and the melt temperature is 185°C to 195°C. Film thickness after corona treatment is 35 µm to 50 µm. Corona treatment to 38 mN/m to 42 mN/m is applied in-line to prepare the surface for solventless lamination to 12 µm PET or 18 µm biaxially oriented polypropylene. Hot tack is tested by ASTM F1921-20; seal strength is tested by ASTM F88/F88M-21. The sealant layer meets FDA 21 CFR 177.1520 paragraph (c) 2.2 and Regulation (EU) No 10/2011 with overall migration below 10 mg/dm². A limitation appears above 180°C seal bar temperature, where butene LLDPE sealant ply shows peel strength decline due to melt thinning and squeeze-out at the seal edge. Converters running wicketed bags at 60 bags/min report that seal bar dwell time must be reduced to 0.2 s to 0.4 s to avoid elongation of the seal perimeter.
Bottle bundles and canned goods shipped in collation shrink film require controlled MD shrinkage to grip container contours and sufficient dart impact to survive cap and rim puncture. A blend of 70 wt% LL 118/21 and 30 wt% LDPE shrink resin with density 0.923 g/cm³ is processed in a high-stalk blown film line with neck height 5 to 8 die diameters above the die, a die gap of 1.6 mm, and a blow-up ratio of 2.5:1. The melt temperature is held at 190°C to 198°C. Frost line height is raised to 600 mm to 800 mm to induce MD orientation. Final film thickness is 50 µm to 60 µm. MD shrinkage at 135°C is characterized by ISO 11501 and should fall within 55% to 70%, while TD shrinkage remains below 25%. Dart impact is measured by ASTM D1709-16a method B, and Elmendorf tear by ASTM D1922-15. The LLDPE component reduces film thickness by approximately 10% to 15% compared with neat LDPE shrink film at equal dart impact, though published data for this specific blend ratio is limited. Operational boundary: if the stalk is lowered below 4 die diameters, MD shrinkage falls below 45% and the film does not conform to bottle caps at the shrink tunnel exit.
Post-consumer recyclate blending in black can liners is confined to 15 wt% because batch-to-batch variation in recyclate melt flow rate shifts bubble stability and creates gel specks visible under transmitted light. LL 118/21 is added at 85 wt% with carbon black masterbatch at 2 wt%. Extrusion on a 70 mm grooved-feed extruder with L/D 24:1 uses a 2.0 mm die gap, a blow-up ratio of 2.0:1 to 2.5:1, and a melt temperature of 190°C to 200°C. Film thickness is 20 µm to 25 µm for 60 L and 100 L garbage liners. Dart impact is measured by ASTM D1709-16a method A for thickness below 25 µm. Elmendorf tear is measured by ASTM D1922-15. The recyclate is sourced from the same blown film line edge trim and is limited to 15 wt% because higher additions reduce bubble cooling and require a drop in line speed of 5% to 10% on 70 mm lines. Heavy metals in the carbon black masterbatch are controlled under EU REACH Annex XVII entry 23 for cadmium and lead. The finished liners are not for food contact.
| Application | LL 118/21 loading (wt%) | Co-resins and additives | Blow-up ratio | Die gap (mm) | End product thickness (µm) |
|---|---|---|---|---|---|
| Frozen food packaging | 70 per skin | 25 LDPE core, 5 HDPE per skin, slip/antiblock 0.4–0.8 | 2.0:1–2.4:1 | 1.8 | 35–45 |
| Heavy-duty sacks | 60 | 25 HMWHDPE, 15 recyclate, 3 CaCO₃ masterbatch | 1.8:1–2.2:1 | 2.0 | 80–100 |
| Agricultural silage wrap | 65–75 per skin | 20 LDPE, 5 mLLDPE, 5 EVOH core, 1 PIB, HALS 0.2 | 2.5:1–3.0:1 | 1.6 | 25–30 |
| Pouch sealant ply | 90 | 10 mLLDPE density 0.912 | 2.2:1 | 1.4 | 35–50 |
| Collation shrink film | 70 | 30 LDPE shrink resin density 0.923 | 2.5:1 | 1.6 | 50–60 |
| Black can liners | 85 | 15 recyclate, 2 carbon black masterbatch | 2.0:1–2.5:1 | 2.0 | 20–25 |
| Application | Regulation/Standard | Test method or clause | Limit or criterion |
|---|---|---|---|
| Frozen food packaging | FDA 21 CFR 177.1520 | Paragraph (c) 2.2 | Olefin polymer for aqueous/acidic/fatty foods under frozen conditions |
| Frozen food packaging | Regulation (EU) No 10/2011 | EN 1186-1 | Overall migration 10 mg/dm² |
| Heavy-duty sacks | ISO 7965-2 | Filled sack drop test | Drop height 1.2 m on face, edge, butt |
| Agricultural silage wrap | ASTM D3985-17 | Oxygen transmission at 23°C, 0% RH | Below 5,000 cm³/(m²·d·atm) |
| Pouch sealant ply | ASTM F1921-20 | Hot tack | Stable seal above 40 m/min |
| Collation shrink film | ISO 11501 | Dimensional change on heating at 135°C | MD 55–70%, TD below 25% |
| Black can liners | EU REACH Annex XVII entry 23 | Cadmium and lead content | Controlled in carbon black masterbatch |
Competitive Braskem LL 118/21 LLDPE Blown Film Extrusion Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Braskem LL 118/21 is a butene-copolymer linear low-density polyethylene supplied in pellet form for blown film extrusion. The resin carries a nominal density of 0.918 g/cm3 when measured under ISO 1183-1/ASTM D792 and a nominal melt flow rate of 2.1 g/10 min at 190 °C/2.16 kg according to ISO 1133-1/ASTM D1238. The combination of a linear backbone and butene short-chain branching produces a semi-crystalline morphology that differs from high-pressure LDPE of the same density by having lower long-chain branching, a narrower molecular weight distribution, and higher elongation at break at equal film gauge. Converters use the grade in industrial sacks, heavy-gauge liners, agricultural tunnels, and blown film layers where seal integrity and tear resistance are more important than high gloss or low haze. The resin is not intended for ultra-clear packaging or for frozen-food stretch film where high dart drop impact at sub-zero temperatures is the controlling property. The shelf life and additive package are controlled by the manufacturer; specific slip and antiblock concentrations should be confirmed on the certificate of analysis before converters adjust winding tension or coefficient-of-friction specifications.
| Property | Value | Test method |
|---|---|---|
| Melt flow rate | 2.1 g/10 min | ISO 1133-1 / ASTM D1238 |
| Density | 0.918 g/cm3 | ISO 1183-1 / ASTM D792 |
| Comonomer type | butene | — |
| Form | pellets | — |
At the molecular level, the butene branch length in LL 118/21 is shorter than the hexene or octene branches used in higher-performance LLDPE film resins, which increases the frequency of chain folding into lamellae during cooling. The consequence is a higher degree of crystallinity at a given density and a lower amorphous tie-chain fraction under high-strain-rate deformation. Differential scanning calorimetry on butene LLDPE of this density class normally shows a broad melting endotherm between 110 °C and 125 °C, with a peak near 122 °C; the exact peak location depends on comonomer distribution and annealing history. The relatively broad endotherm supports heat-sealing behaviour but limits dimensional stability when the film is exposed to temperatures above 50 °C under tension. Because the resin is polymerised in a low-pressure gas-phase or solution process rather than an autoclave LDPE process, long-chain branching is minimal; this is the main structural reason for lower melt strength and more rapid bubble instability at high blow-up ratio.
Extrusion trials on grooved-feed blown film equipment with 25:1 to 30:1 L/D screws indicate that melt temperatures between 190 °C and 220 °C give a stable bubble with moderate back pressure. At screw speeds above 90 rpm on 75 mm extruders, melt temperature can rise above 230 °C, at which point the residence time should be limited to avoid oxidative gel formation. The die gap is normally set between 1.5 mm and 2.5 mm; die gaps below 1.2 mm increase shear stress at the lip and may push the melt into sharkskin melt fracture at high output. Blow-up ratios are typically held at 2.0:1 to 3.0:1, with the lower half of that range favouring machine-direction tensile strength and the upper half favouring transverse-direction tear balance. Internal bubble cooling can be used to raise output, but a frost line height below 500 mm may freeze orientation before sufficient transverse-direction relaxation, producing an unbalanced film. These ranges are line-dependent and should be adjusted on the basis of die diameter, air ring geometry, and ambient air temperature.
Compared with metallocene-catalysed hexene or octene LLDPE grades of the same 0.918 g/cm3 density, LL 118/21 typically exhibits lower dart drop impact and lower puncture resistance because the butene branch is shorter and less effective at disturbing crystallinity under rapid deformation. In exchange, the resin can be processed on older blown film lines with less pressure sensitivity and does not require the tighter temperature and die-gap control that some mLLDPE grades demand. Against high-pressure LDPE, LL 118/21 shows higher tensile elongation and dart impact at equivalent gauge, but lower melt strength and a narrower neck-in window during air-cooled tubular extrusion. Seal initiation temperature is generally higher for butene LLDPE than for hexene or octene LLDPE, but the plateau is wider because of the broad comonomer distribution, which can help package seals after hot filling if the dwell time is sufficient. The difference is not absolute; converter film properties depend strongly on draw-down ratio, frost line height, and film thickness.
Film property measurements are reported according to ASTM D882 for tensile properties, ASTM D1922 for Elmendorf tear, and ASTM D1709 for dart drop impact. Because nominal values are thickness-dependent, mechanical comparison between grades is meaningful only at the same gauge, same blow-up ratio, and same conditioning protocol under 23 °C and 50 % relative humidity. The moisture vapour transmission rate is not a resin property alone; it depends on film thickness and is commonly measured by ASTM F1249 or ISO 15106-2. Similarly, oxygen transmission rate should be reported under ASTM D3985 or ISO 15105-2, and converters should avoid comparing barrier data obtained at different relative humidity levels because polyethylene is not a high-barrier polymer and its gas transport properties are sensitive to temperature.
Tear strength in LL 118/21 film is controlled by orientation. At a constant die gap and melt temperature, raising blow-up ratio from 2.0:1 to 3.0:1 increases transverse-direction Elmendorf tear and reduces machine-direction tear; raising frost line height increases machine-direction orientation and raises machine-direction tensile yield stress. A die gap reduction to 1.5 mm at high output increases machine-direction orientation and may produce a film with high machine-direction tear but low dart drop impact because the film absorbs less energy before puncture. Producers of heavy-duty sacks often run thicker dies and moderate blow-up ratio to preserve dart impact, while producers of carrier bags accept some loss in dart impact to gain machine-direction stiffness. The relationship is not linear because increasing die gap also lowers shear stress and may delay the onset of sharkskin melt fracture, allowing higher output before surface defects appear.
Capillary rheometry on butene LLDPE in the MFR 2.1 g/10 min class indicates shear thinning with a power-law index in the range 0.5–0.6 at 190 °C; this means that apparent viscosity falls more slowly with shear than in broad-molecular-weight-distribution LDPE. Therefore, at high screw speeds, the pressure drop across the die is more sensitive to die gap than to melt temperature. The temperature coefficient of viscosity is lower than for LDPE; operators who raise the melt temperature to reduce extruder load often generate only marginal pressure reduction while increasing oxidation risk. Melt pump systems are recommended when the die gap is kept above 2.0 mm and blow-up ratio exceeds 2.5:1 to stabilise downstream gauge variation; without a melt pump, screw-induced pressure pulsations can produce gauge bands in thicker films. The melt extensibility during bubble expansion is lower than for LDPE, so the bubble must be supported by a stable air ring and, where necessary, internal bubble cooling; otherwise a fluttering bubble creates periodic gauge variation.
On a 300 mm die with dual-lip air ring and no internal bubble cooling, stable operation is commonly reported at 1.8 mm die gap, melt temperature 205 °C, blow-up ratio 2.4:1, and frost line height 700 mm. Raising output until bubble flutter appears often corresponds to a draw-line conflict rather than a resin deficiency; the flutter can be suppressed by lowering the lower air ring or increasing the upper ring velocity. When the same bubble is run at blow-up ratio 3.2:1, the transverse-direction-to-machine-direction tear ratio shifts above 1.2:1, but gross output may become limited by bubble contact with the upper cage. These observations are line-specific; converters should not transfer settings directly from a different die diameter without rechecking the frost line height and symmetric bubble dimension.
Heat-seal initiation for butene-copolymer LLDPE is generally higher than for hexene or octene copolymers of the same density. The difference is attributable to the limited branch length of butene, which yields a more orderly crystalline surface at the seal interface and requires more thermal energy to reach the melt state. In packaging lines where sealing jaws run above 130 °C, the practical difference may be negligible; in low-temperature sealing applications, the gap can be 5–15 °C depending on film gauge and contamination. Seal strength is measured under ASTM F88/F88M, seal initiation under ASTM F2029, and hot-tack force under ASTM F1921. LL 118/21 is used in lamination layers where seal strength is dominated by the sealing layer thickness and the thermal mass of the jaw; converters should verify hot-tack window on the target machine because published data for this specific configuration is limited.
Industrial liners made from LL 118/21 are typically blown at 100–200 µm gauge and evaluated for puncture resistance under ASTM D5748 and tensile toughness under ASTM D882. Agricultural greenhouse films may include UV stabilisation in masterbatch; the base resin is not supplied with UV additives unless the manufacturer’s specification states otherwise. Liquid packaging liners require organoleptic testing according to packaging converter protocols; low residual odour and taste are not automatically guaranteed and should be confirmed under DIN 10955 or equivalent sensory methods. Frozen food films are outside the preferred performance envelope unless the film is thick enough to compensate for the lower sub-zero dart impact of butene copolymers compared with C6/C8 LLDPE.
LL 118/21 can be blended with LDPE to increase melt strength and improve bubble stability, or with HDPE to raise stiffness and moisture barrier, but the blend properties do not follow a linear mixing rule. At 10–20 % LDPE addition, dart drop impact is usually retained while neck-in decreases; at 30 % HDPE addition, stiffness increases but machine-direction Elmendorf tear may decrease sharply because of the reinforcing immiscible HDPE lamellae. The blending step should be performed with a separate dosing system rather than tumble mixing alone; segregation during pellet transfer can generate concentration drift along the bubble. The use of a high-shear mixer is not required for these polyolefin blends if the screw contains a distributive mixing section of 8–10 D length.
For food-contact use, the olefin base polymer is generally listed under FDA 21 CFR 177.1520(c) for olefin polymers, with specific end-use limitations determined by temperature and food type; the supplier’s food-contact statement governs whether LL 118/21 meets a given condition of use. Under EU 10/2011, the overall migration limit for plastic materials and articles is 10 mg/dm2 for standard food simulants, and the specific migration of any additive in the formulation must be confirmed against the union list. REACH candidate list substances are reported below the 0.1 % w/w threshold. RoHS compliance is not usually a limiting issue for unfilled polyethylene film; however, converters selling into electrical and electronic applications should verify brominated flame retardant content because additive packages differ by lot. These statements are conditional and do not replace a certificate of compliance from Braskem.
| Regulation / standard | Scope | Verification condition |
|---|---|---|
| FDA 21 CFR 177.1520(c) | Olefin polymers in food-contact articles | Supplier food-contact statement and end-use temperature/food-type limits |
| EU 10/2011 | Plastic materials and articles intended for food contact | Overall migration limit 10 mg/dm2 |
| REACH | Candidate list substances in articles | Reported below 0.1 % w/w |
| RoHS | Restricted substances in electrical and electronic equipment | Verify additive package for brominated flame retardants |
Polyethylene melt enters oxidative degradation if the extruder stops with a hot barrel above 180 °C; the formation of crosslinked gel particles depends on residence time and antioxidant consumption. When changing from LL 118/21 to a lower-viscosity HDPE, converters typically purge with a lower-MFR LDPE or a commercial purge compound at a barrel temperature of 180–200 °C. The use of high-shear screws with mixing elements disperses gels but does not dissolve them; upstream filtration through 60–100 mesh screen packs is standard on film lines to trap degraded particles. No halogenated purge agents should be used unless subsequently cleared with a commercial purging compound, because additive residues can affect film colour and seal odour.
Pellets should be stored in a dry area below 50 °C and protected from ultraviolet exposure. Moisture absorption is negligible at ambient humidity; pre-drying is unnecessary unless condensed water is present on pellet surfaces from temperature cycling. Water on the pellet surface can produce surface streaks or splay in cast film but is not a typical blown film failure. If condensation is observed, a hopper dryer at 60–70 °C for 1–2 h may be used. Conveying systems should avoid long-radius bends that generate angel hair; angel hair can survive the extruder throat and appear as gels in the film.
Slip and antiblock additives are formulated into the resin to control film-to-film friction and blocking during winding. If the converter builds a structure with an outer layer of LL 118/21 and a core layer of HDPE, the slip additive migration rate is finite; blocking can occur in warehouse storage above 35 °C before additive bloom equilibrates. Coefficient of friction is measured under ISO 8295 or ASTM D1894. Film-to-film blocking is not fully captured by the standard static coefficient-of-friction test; storage trials at 40 °C and 70 % relative humidity for 48–72 h are used during qualification.