| HS Code | 258803 |
| Density | 0.922 g/cm³ |
| Melt Flow Rate 190 C 2 16 Kg | 0.7 g/10 min |
| Tensile Strength At Yield Md | 10 MPa |
| Tensile Strength At Break Md | 35 MPa |
| Elongation At Break Md | 800% |
| Dart Impact Strength | 150 g |
| Elmendorf Tear Strength Md | 200 g |
| Elmendorf Tear Strength Td | 300 g |
| Haze | 12% |
| Gloss 45 | 60 |
| Melting Point | 122°C |
| Vicat Softening Point | 100°C |
| Coefficient Of Friction | 0.2 |
| Blocking | Low |
| Thermal Stability | Good |
As an accredited Braskem HF2207B5 Blown Film Extrusion Linear Low Density Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Braskem HF2207B5 Blown Film Extrusion Linear Low Density Polyethylene supplied in 25 kg polyethylene bags, palletized and stretch-wrapped. |
| Container Loading (20′ FCL) | Braskem HF2207B5 LLDPE blown film extrusion resin loaded in a 20-foot FCL container, palletized bags, dry conditions, fully secured cargo. |
| Shipping | Braskem HF2207B5 Blown Film Extrusion Linear Low Density Polyethylene is a non-hazardous resin. It is shipped in 25 kg bags or bulk bags, palletized and stretch-wrapped. Transport in clean, dry trucks/containers. Protect from moisture, heat, UV, and contamination. Keep containers closed. Not regulated by DOT, IMDG, or IATA. |
| Storage | Store Braskem HF2207B5 LLDPE in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, flames, and strong oxidizing agents. Keep bags or containers closed, clean, and palletized off the floor to prevent moisture and contamination. Avoid prolonged UV exposure and excessive stacking. Follow supplier SDS and local regulations for safe handling and storage. |
| Shelf Life | No specific shelf life; stable if stored unopened in a cool, dry, well-ventilated area away from direct sunlight and heat. |
Film widths above 1,500 mm for industrial liners and heavy-duty sacking impose a narrow processing window on Braskem HF2207B5, a blown film extrusion linear low density polyethylene with nominal density of 0.922 g/cm³ under ISO 1183-1 and melt mass-flow rate of 1.0 g/10 min under ISO 1133-1. Monolayer lines equipped with 250–350 mm spiral mandrel dies and 2.0–2.4 mm die gaps run the resin at melt temperatures of 190–210 °C; output stability degrades rapidly above 220 °C due to oxidation, while below 185 °C melt strength is insufficient to hold a consistent bubble at high stalk. On older LDPE lines with 0.7–1.0 mm die gaps, shark-skin melt fracture appears unless the gap is opened to 2.0 mm or greater; this is the most common production bottleneck reported by converters moving from LDPE shrink film to LLDPE heavy-duty sacks. The addition ratio places HF2207B5 at 70–85 wt% of the extruder feed, with 15–30 wt% LDPE of 0.923–0.924 g/cm³ density introduced to restore bubble stability when internal bubble cooling is absent. On newer lines with dual-lip air rings and internal bubble cooling, 100 wt% HF2207B5 is feasible, but frost line height must be maintained within ±10 mm of the setpoint to avoid film thickness variation of more than ±5% across the web. Slip concentrate is added at 500–800 ppm erucamide and antiblock at 800–1,200 ppm synthetic silica to prevent blocking after gusseting; exceeding 1,500 ppm synthetic silica reduces dart impact under ASTM D1709A to levels that frequently fail drop-filled sack specifications. Compliance for non-food industrial liners is governed by purchase-specification standards rather than a single regulation: ASTM D638 for tensile yield and break, ASTM D1709A for dart drop, ASTM D1922 for Elmendorf tear, and ASTM D5748 for puncture propagation resistance. Terminal products include flat-bottom sacks for resin pellet transfer, drum liners for paints and coatings, and gusseted liners for construction powders, cement, and mineral fillers.
Stretch hood film production with Braskem HF2207B5 places the resin at 85–100 wt% of the formulation; the balance is an LDPE of 0.924 g/cm³ density when converters must damp machine-direction stretch recovery and improve bubble stability on collapsing frames with long gussets. Processing uses a 200–300 mm die, a die gap of 2.0–2.6 mm, melt temperature of 185–205 °C, and blow-up ratio of 2.0:1–2.3:1; the lower end of the blow-up range is maintained because transverse direction orientation in stretch hood film must not exceed machine direction orientation, or the hood will not recover uniformly over pallet corners. Frost line height is set at 2–3 times the die diameter, and the collapsing frame angle is typically 20–30°; field failures on production lines occur as gusset wrinkles when the frame is misaligned by more than 1.5°, producing local thickness reductions of 10–15% that initiate tears during pallet transport. The formulation omits slip additive, because surface migration of erucamide reduces the friction required to hold the hood on the pallet and can cause creep; antiblock is held at 500 ppm or less. Acceptance testing references ISO 527-3 for tensile properties and ASTM D882 for machine-direction and transverse-direction break, with some converters specifying a 100% elongation recovery test at 23 °C after 60 min relaxation; published data for this specific configuration is limited and must be established by converter trial. Terminal products include stretch hoods for palletized beverage, appliance, and construction board loads, where film thickness is typically 50–80 µm.
A monolayer structure used for primary food bags places Braskem HF2207B5 at 100 wt% of the extruder feed; in three-layer coextrusions, the grade is positioned as the sealant skin at a layer ratio of 20–30% of total film thickness, while the core and outer skin may contain metallocene LLDPE, HDPE, or a barrier tie resin depending on the required oxygen transmission rate. The addition of slip concentrate is limited to 400–800 ppm erucamide and antiblock to 600–1,000 ppm synthetic silica; higher loadings reduce seal strength and increase haze, and slip migration into seal interfaces at above 800 ppm can lower hot-tack strength at packaging speeds above 60 packs/min. Blown film processing for this sector uses a die gap of 1.8–2.2 mm, melt temperatures of 180–200 °C, and a blow-up ratio of 2.0:1–2.4:1; the bubble is kept short to preserve optical clarity and reduce blocking tendency. Direct food-contact compliance is anchored to FDA 21 CFR 177.1520(c) olefin polymer requirements and EU 10/2011 Annex I and II migration limits; converters verify overall migration under EN 1186 and specific migration of additives under EN 13130. Terminal products include frozen vegetable bags, cereal liners, bakery bread bags, and primary pouches for dry powders.
| Compliance obligation | Standard / clause | Verification method | Application boundary |
|---|---|---|---|
| U.S. direct food contact | FDA 21 CFR 177.1520(c) | Extraction per FDA 21 CFR 176.170 | All food types under Conditions of Use A–H unless stated |
| EU plastics food contact | EU 10/2011 Annex I and II | Overall migration per EN 1186, specific migration per EN 13130 | Dry and aqueous foods; fatty foods require specific migration evaluation |
| GMP for food-contact materials | EC 2023/2006 | Quality system audit | Converter responsibility |
Dart impact retention in agricultural silage covers made from Braskem HF2207B5 is governed by additive dispersion and by the interaction between carbon black and hindered amine light stabilizers; the polymer alone does not withstand ultraviolet exposure beyond short service intervals. The formulation constitutes HF2207B5 at 96.5–97.5 wt% of the finished compound, with active carbon black loading at 2.0–2.5 wt%, hindered amine light stabilizer at 0.30–0.60 wt%, and processing antioxidant at 0.05–0.10 wt%. The extrusion operation uses blown film lines with die gaps of 1.8–2.4 mm, melt temperatures of 190–210 °C, and blow-up ratios of 2.0:1–2.4:1; film thickness is commonly 150–250 µm, and widths reach 8–12 m on large agricultural lines with internal bubble cooling. The primary mechanical failure mode in service is cracking at fold creases, where localized stress whitening reduces dart impact even when bulk film properties remain within specification; converters therefore inspect fold-zone tear resistance under ASTM D1922 after repeated flexing. The applicable industry compliance framework is EN 13206:2017 for thermoplastic covering films used in agriculture and horticulture, with additional tensile verification under ISO 527-3. Terminal products include silage bags, tunnel covers, greenhouse side curtains, and temporary fumigation covers.
| Technical boundary | Standard | Measured parameter | Application condition |
|---|---|---|---|
| Agricultural covering film classification | EN 13206:2017 | Thickness, width, optical and thermal properties | Silage bags, tunnel covers, greenhouse cladding |
| Tensile behavior of film | ISO 527-3 | MD/TD stress at yield and break | 23 °C, 50% RH |
| Dart impact resistance | ASTM D1709A | Failure mass of conditioned film | New film and flexed fold-zone specimens |
Corona-treating a blown sealant web made from Braskem HF2207B5 to a surface energy of 40–44 mN/m is the first step in adhesive lamination to printed polyester or biaxially oriented polypropylene. The sealant layer is run at 100 wt% HF2207B5 or at 70–80 wt% HF2207B5 with 20–30 wt% LDPE when the end-use requires a lower seal initiation temperature and shorter dwell time on high-speed form-fill-seal machines. Slip and antiblock are held lower than in monolayer industrial film: erucamide at 400–600 ppm, synthetic silica at 500–800 ppm. Higher slip levels migrate to the film surface after corona treatment and reduce lamination bond strength measured under ASTM F904, while excessive antiblock increases haze and interferes with seal integrity. Blown film processing uses a die gap of 1.6–2.0 mm, melt temperatures of 180–200 °C, and film thickness of 40–70 µm; after slitting and corona treatment, lamination with solventless polyurethane adhesives is performed at typical coating weights of 2.0–3.0 g/m². Compliance for the sealant layer is anchored to FDA 21 CFR 177.1520(c) and EU 10/2011, with seal strength verified under ASTM F88/F88M. Terminal products include stand-up pouches, pillow pouches, sachets, and lidding webs for dry and moist food applications.
Sub-slab barrier membranes made from Braskem HF2207B5 are produced as monolayer blown film at thicknesses of 300–500 µm, with the polymer fed at 100 wt% and carbon black masterbatch added to reach an active carbon black concentration of 2.0–3.0 wt% for opacity and long-term soil-contact stability. The extrusion line uses a die gap of 2.0–2.5 mm, melt temperatures of 190–210 °C, and a blow-up ratio of 1.6:1–2.0:1; the low blow-up ratio biases orientation toward machine direction tensile, which is required for puncture resistance over aggregate and irregular substrates. Widths up to 6–8 m are produced on high-output lines with internal bubble cooling; gusseting is avoided because folded edges create stress concentrations that reduce gas barrier consistency. The relevant compliance framework is EN 13967:2012 for flexible sheets for waterproofing and ASTM E1745 for water vapor retarders used under concrete slabs; gas-permeability testing may be specified under ASTM D1434 for radon diffusion evaluation. Field installation failure modes include puncture by angular aggregate and seam separation; converters therefore specify tensile properties under ISO 527-3 and puncture resistance under ASTM D5748. Terminal products include radon barriers, moisture vapor retarders, and gas membranes placed beneath concrete floor slabs or inside crawl-space envelopes.
Competitive Braskem HF2207B5 Blown Film Extrusion Linear Low Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Braskem HF2207B5 is a blown film extrusion linear low density polyethylene resin supplied as pelletized butene-based linear low density polyethylene. The grade is manufactured through a gas-phase polymerization route and is intended for monolayer and coextruded film structures. Nominal density is 0.922 g/cm³ when measured according to ASTM D1505, and nominal melt flow rate is 0.70 g/10 min at 190°C/2.16 kg under ASTM D1238. The product designation identifies a film extrusion grade with butene comonomer incorporation and a stabilizer package configured for blown film processing. Published technical documentation positions HF2207B5 for applications requiring a balance between dart impact resistance, seal integrity, and moderate optical properties in polyethylene film.
Molecular architecture consists of linear polyethylene chains with short-chain branches introduced by the butene comonomer. The molecular weight distribution is broader than that of solution-phase metallocene LLDPE but narrower than that of high-pressure low density polyethylene. Differential scanning calorimetry conducted at 10°C/min per ASTM D3418 typically indicates a peak melting temperature between 123°C and 126°C and a peak crystallization temperature between 107°C and 110°C. The density of 0.922 g/cm³ reflects a reduced crystalline fraction relative to high density polyethylene, which lowers modulus and allows film to be drawn at higher blow-up ratios without splitting under normal conditions. Because the resin is linear rather than long-chain branched, it develops less extensional strain hardening than high-pressure LDPE and therefore requires more controlled bubble cooling during extrusion.
The additive package is recorded on the lot-specific certificate of analysis rather than in generic technical literature. It typically includes processing stabilizers, antioxidant, and neutralizer components. The resin does not require pre-drying under closed-pellet storage at relative humidity below 60%. Above that threshold, surface moisture can generate splay and bubble destabilization on blown film lines. Slip and antiblock additives, where needed, are generally introduced by converter-added masterbatch rather than as part of the base stabilizer system.
On smooth-bore blown film extruders with L/D ratios between 24:1 and 30:1, melt temperature measured at the die is commonly held between 195°C and 230°C. Grooved-feed extruders permit higher output rates because the linear backbone does not produce the same degree of screw slip as high-pressure LDPE. A die gap of 1.5 mm to 2.5 mm is typical for this density range. Narrower gaps increase shear rate and can promote melt fracture, while wider gaps require additional cooling capacity to maintain a stable frost line. Blow-up ratios between 2.0:1 and 3.0:1 are used commercially for this resin class. Frost line heights of 6 to 10 die diameters provide a balance between bubble stability and optical quality, although the optimum position depends on air-ring design and ambient humidity.
The linear chain structure produces a shear-thinning response that is lower in magnitude than that of high-pressure LDPE. Apparent viscosity decreases less sharply at high screw speeds, so melt-temperature override can occur if extruder screw speed is increased without adjusting barrel temperatures. On a 40 mm extruder with L/D 30:1 and a barrier screw, specific energy consumption is generally 0.18 kWh/kg to 0.24 kWh/kg. Higher values indicate excessive shear heating and should be corrected by reducing screw speed or raising rear barrel temperature. Head pressure is typically maintained below 35 MPa; pressure fluctuations above 2 MPa per hour suggest feed instability or melt-temperature variation.
Melt temperature is limited primarily by the onset of thermal oxidative degradation and loss of bubble stability, not by the crystalline melting point. At melt temperatures above 240°C, antioxidant consumption accelerates, and film extruded at the die lip can exhibit gel formation, edge instability, and reduced dart impact after post-treatment. The butene branches are less thermally sensitive than the higher alpha-olefin branches in some metallocene resins, but accumulated heat history across multiple extrusions shifts the degradation onset lower. In production-scale monolayer lines, extruder barrel temperatures are set in a decreasing profile from 190°C at the feed throat to 220°C at the adapter and 210°C to 225°C at the die. These settings maintain melt homogeneity without exceeding the thermal oxidation threshold.
Bubble stability is also affected by frost line drift. A frost line position that oscillates by more than ±1 die diameter indicates inadequate air-ring control or fluctuating internal bubble pressure. Lines equipped with internal bubble cooling can increase output by 15% to 25% relative to natural cooling, but internal bubble pressure must remain below 500 Pa to prevent bubble flapping. On air-cooled lines, the distance from the die face to the frost line should be stable before film property sampling; property variation is often traceable to changing frost line height rather than raw resin lot variation.
Film performance at 25 µm thickness is governed by draw ratio, blow-up ratio, and cooling rate. Typical laboratory film produced on a 40 mm blown film line with a 2.5:1 blow-up ratio is evaluated for dart impact, tear, tensile, haze, and gloss. A representative range for dart drop impact is 90 g to 130 g using ASTM D1709/A. Machine-direction Elmendorf tear is typically 180 gf to 260 gf, and transverse-direction tear is typically 240 gf to 340 gf, both measured under ASTM D1922. Tensile yield strength per ASTM D882 is 11 MPa to 13 MPa in both machine and transverse directions. Elongation at break is commonly above 700%. These values shift with gauge, blow-up ratio, and cooling rate; they are indicative industrial film data rather than specification limits.
Optical performance is moderate rather than premium because the 0.922 g/cm³ density produces larger crystalline structures than metallocene grades. Haze on 50 µm film is typically 8% to 12% per ASTM D1003, and 45° gloss is typically 45 to 60 per ASTM D2457. The addition of synthetic silica antiblock masterbatch at 3 wt% to 5 wt% can raise haze by 1 to 3 percentage points and lower gloss by 3 to 8 units. This trade-off is relevant in form-fill-seal operations where film-to-film slip is required on vertical surfaces.
| Film property at 25 µm unless noted | HF2207B5 typical range | Conventional 0.918 g/cm³ butene LLDPE | Octene mLLDPE 0.918 g/cm³ |
|---|---|---|---|
| Dart drop impact, ASTM D1709/A | 90–130 g | 70–110 g | 150–300 g |
| MD Elmendorf tear, ASTM D1922 | 180–260 gf | 150–250 gf | 100–180 gf |
| TD Elmendorf tear, ASTM D1922 | 240–340 gf | 220–320 gf | 180–280 gf |
| Haze on 50 µm, ASTM D1003 | 8–12% | 10–15% | 2–5% |
| Gloss at 45°, ASTM D2457 | 45–60 | 40–55 | 70–90 |
| Seal initiation at 5 N/25 mm | 104–108°C | 102–106°C | 88–95°C |
Heat-seal performance is normally tested on a laboratory heat sealer with 0.5 MPa jaw pressure and 0.5 s dwell. Seal initiation temperature defined at 5 N/25 mm is in the range of 104°C to 108°C for 38 µm film. Hot-tack strength is lower than that of high-pressure LDPE containing long-chain branching and lower than that of plastomer-based LLDPE. In high-speed vertical form-fill-seal machines, this difference can require an increase in sealing temperature of 5°C to 8°C or an increase in dwell time of 50 ms to 100 ms. Published data for this specific grade on high-speed horizontal form-fill-seal lines is limited; converter trial confirmation is required for packaging validation.
The higher density of 0.922 g/cm³ produces measurable changes in film stiffness, blocking resistance, and seal initiation temperature. In a down-gauged liner from 50 µm to 38 µm, tensile yield strength typically increases by 5% to 10% relative to a 0.918 g/cm³ butene LLDPE at the same melt flow rate. This permits gauge reduction without loss of load-bearing capacity in the transverse direction. However, the higher density also raises seal initiation temperature by approximately 1°C to 2°C and can reduce hot-tack strength if sealing jaw dwell time is not increased. The difference from octene-based metallocene LLDPE is more pronounced: the metallocene grade retains higher dart impact at lower gauge and provides lower seal initiation, but often requires lower melt temperature to avoid bubble instability on older monolayer lines.
Compared with high-pressure LDPE, HF2207B5 gives higher dart impact and puncture resistance at equal gauge but lower melt strength. In blends with LDPE, addition of 10 wt% to 30 wt% LDPE is used to increase bubble stability and improve optical properties. The linear structure reduces shear thinning relative to LDPE, so extruder motor load on smooth-bore extruders may rise when HF2207B5 is run at the same output. This operational boundary is most evident on machines with L/D 24:1 and no grooved feed. Converters using such machines without increasing barrel temperatures may observe lower throughput or higher melt temperature instead of improved film toughness.
The difference from conventional butene LLDPE at 0.918 g/cm³ is primarily a density-driven increase in modulus and a modest loss in low-temperature impact. In frozen food applications, the low-temperature brittleness of linear low density polyethylene is better than high-pressure LDPE. The butene branch distribution provides sufficient tie molecules to prevent brittle failure at -40°C when gauge is above 25 µm. At gauge below 20 µm, dart impact may decrease sharply; converter-reported data for this specific thickness is limited, and laboratory film data should not be extrapolated without production-scale verification.
In coextruded film structures, HF2207B5 can serve as a core or outer layer in three-layer and five-layer constructions. In a five-layer agricultural silage film, the grade may be placed in the core to contribute melt strength while an ethylene-vinyl acetate or metallocene plastomer forms the sealing layer. Bubble stability in this configuration is maintained by setting the HF2207B5 extruder temperature profile 5°C to 10°C lower than the outer LDPE extruder to compensate for viscosity mismatch. This is not a specification, but an operational setting reported on production lines with 50 mm coextrusion barrier screws. The resin is not optimized for cast film or extrusion coating. The absence of long-chain branching limits draw resonance control in cast processes, and published data for cast film use of this specific grade is limited.
| Regulatory or standard reference | Relevant clause or method | Application note |
|---|---|---|
| FDA 21 CFR 177.1520 | (c) 3.1a/3.2a | Olefin polymer provisions; finished article migration testing required |
| EU Regulation (EU) No 10/2011 | Annex I, overall migration limit 10 mg/dm² | Compliance depends on thickness, time, and temperature |
| REACH (EC) No 1907/2006 | Article 33 SVHC communication | No SVHC above 0.1 wt% in supplied form |
| RoHS 2011/65/EU | Annex II restricted substances | Not usually applicable to polymer film, but supply chain verification recommended |
| CONEG | Sum of Pb, Hg, Cd, Cr6+ below 100 ppm | Heavy-metals limit verified by supplier |