Braskem Green Pe Sll218 Blow Film Extrusion And Cast Film Extrusion Linear Low Density Polyethylene

Braskem Green PE SLL218 Blow Film Extrusion and Cast Film Extrusion Linear Low Density Polyethylene

    • Product Name: Braskem Green PE SLL218 Blow Film Extrusion and Cast Film Extrusion Linear Low Density Polyethylene
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 465768
    Product Name Braskem Green PE SLL218
    Manufacturer Braskem
    Polymer Type Linear Low Density Polyethylene (LLDPE)
    Renewable Source Sugarcane ethanol
    Applications Blow Film Extrusion and Cast Film Extrusion
    Density 0.918 g/cm³
    Melt Index 190 C 2 16 Kg 1.0 g/10 min
    Melting Point 121 °C
    Vicat Softening Point 100 °C
    Tensile Strength At Break 25 MPa
    Elongation At Break 800 %
    Flexural Modulus 200 MPa
    Dart Drop Impact 120 g
    Elmendorf Tear Strength Md 200 g
    Elmendorf Tear Strength Td 300 g
    Haze 10 %
    Gloss 45 70
    Coefficient Of Friction 0.20
    Seal Initiation Temperature 105 °C
    Processing Temperature 160-210 °C
    Blow Up Ratio 2.0-3.0
    Film Thickness 20-100 µm
    Antiblock Yes
    Slip Yes
    Renewable Content 100 %

    As an accredited Braskem Green PE SLL218 Blow Film Extrusion and Cast Film Extrusion Linear Low Density Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing Braskem Green PE SLL218 is packaged in 25 kg polyethylene bags, 40 bags per stretch-wrapped pallet, totaling 1,000 kg.
    Container Loading (20′ FCL) Container Loading (20′ FCL): Braskem Green PE SLL218 LLDPE resin, 25 kg palletized bags, shrink-wrapped, loaded for blow/cast film extrusion.
    Shipping Braskem Green PE SLL218 is shipped as non-hazardous LLDPE pellets in 25 kg bags or 1,000 kg bulk octabins, palletized and stretch-wrapped. Transport in clean, dry vehicles/containers at ambient temperature. Keep dry, avoid direct sunlight, heat, moisture, and contamination. Handle with care to prevent package damage. Follow local regulations.
    Storage Store Braskem Green PE SLL218 indoors in a cool, dry, well-ventilated area away from direct sunlight, heat, ignition sources, and strong oxidizers. Keep bags/containers tightly closed, palletized, and off the floor to prevent moisture and contamination. Protect from UV, dust, and temperature extremes. Follow the manufacturer’s SDS and local storage regulations. Use first-in, first-out stock rotation. Inspect containers regularly.
    Shelf Life Shelf life is 12 months from manufacture when stored unopened in a cool, dry, well-ventilated area away from direct sunlight.
    Application of Braskem Green PE SLL218 Blow Film Extrusion and Cast Film Extrusion Linear Low Density Polyethylene

    On a three-layer cast film extrusion line equipped with a 2,400 mm coat-hanger die, a 0.8 mm die slot, and vacuum box edge pinning, Braskem Green PE SLL218 is introduced as the core layer at 100 wt% with melt pump discharge pressures between 85 bar and 110 bar. The nominal melt flow rate of the grade is 1.0 g/10 min at 190 °C/2.16 kg per ISO 1133-1:2022, and nominal density is 0.918 g/cm³ per ISO 1183-1. The outer layers are metered at 10 wt% to 15 wt% of total structure; per 100 parts of SLL218 in each skin layer, 3–5 phr of polyisobutylene cling masterbatch and 5–8 phr of LDPE with a melt index of 1.8 g/10 min are added to stabilise the melt curtain and control cling force. Melt temperatures at each extruder adapter are held between 238 °C and 250 °C, while the polished chrome chill roll is maintained at 22 °C to 28 °C; chill roll temperatures below 18 °C induce differential surface crystallisation that manifests as machine-direction curl and gauge bands at line speeds above 350 m/min. Air gap between die lip and chill roll contact is set at 18 mm to 25 mm. Film thickness for machine wrap runs from 12 μm to 17 μm, while hand wrap runs from 18 μm to 23 μm. In-line edge trim is recycled into the core layer at 5 wt% to 8 wt% without measurable gel formation when extruder screw speed is held at or below 110 rpm. Cling force is measured according to ASTM D5458 and maintained at 80 g to 120 g for a 500 mm sample width; tensile elongation at break is evaluated per ISO 527-3 with specimens conditioned at 23 °C ± 2 °C and 50 % ± 5 % relative humidity. The terminal article is a pallet-stabilising stretch wrap for non-direct food contact logistics; where incidental food contact is declared, the cling masterbatch and skin layer must be validated under FDA 21 CFR 177.1520 and EU Regulation No 10/2011 for overall migration below 10 mg/dm². Thermal stability of the PIB cling additive in the skin layer becomes limiting above 260 °C, producing smoke and deposit on the casting roll; during short stops the melt temperature should therefore be reduced to 180 °C.

    When Silage Film Oxygen Ingress Exceeds 1400 cm³/m²·day·atm at 25 °C

    Blown silage wrap produced from SLL218 is typically extruded on a monolayer or three-layer blown film line with die diameter between 200 mm and 350 mm, die gap from 1.8 mm to 2.4 mm, and blow-up ratio set between 2.2 and 3.0. Melt temperature measured at the die head is held from 190 °C to 215 °C; frost line height is maintained at 4 to 6 die diameters to prevent excessive machine-direction orientation without sacrificing transverse-direction tensile. The formulation for a monolayer silage grade uses 100 parts SLL218, 10–15 phr LDPE, 4–6 phr carbon black masterbatch with aggregate particle size from 17 nm to 25 nm, 0.3–0.5 phr HALS UV stabiliser, and 0.1–0.2 phr polymer processing aid. Carbon black loading is determined by opacity and weathering requirements; below 4 phr, UV screening in 12-month outdoor exposure becomes insufficient, while above 6 phr the film surface roughness raises coefficient of friction above 0.45 by ISO 8295, causing baler tracking issues. Oxygen transmission rate is measured by ASTM D3985 at 23 °C and 0 % RH; converter specifications for silage barrier commonly require OTR below 1400 cm³/m²·day·atm for a 25 μm film. Thickness for silage wrap is typically 25 μm to 40 μm, and roll width is 750 mm or 1500 mm; the terminal article is a stretch wrap used around grass, maize, or whole-crop silage bales for anaerobic fermentation. Mechanical integrity is evaluated through puncture resistance per ASTM D5748 and dart impact per ASTM D1709 Method A. Compliance for the film falls under EU REACH and the absence of Substances of Very High Concern; where the film contacts wet acidic silage leachate, extraction of additives under EU Regulation No 10/2011 simulant B should be verified. Process limitation: at blow-up ratios below 2.0, transverse-direction tear strength declines to levels that allow splitting at baler friction points, and film yield stress in the machine direction increases sufficiently to cause irregular pre-stretch on bale wrappers.

    Heavy-duty form-fill-seal sack lines running SLL218 in a three-layer blown configuration often demand a film thickness of 70 μm to 130 μm and a die gap of 2.0 mm to 2.5 mm to compensate for low melt strength. The layer ratio is maintained at 30/40/30, with the core containing 15–20 phr LDPE to increase bubble stability and the outer layers containing 0.2–0.4 phr slip/antiblock masterbatch. During extrusion, barrel temperatures are profiled from 170 °C at the feed throat to 210 °C at the die, and internal bubble cooling is used to raise output above 250 kg/h on lines with 85 mm extruder screw diameter and 30:1 L/D. The resultant film is converted into heavy-duty shipping sacks for resin granules, fertiliser, and construction powders on form-fill-seal equipment, where seal strength measured by ASTM F88 must remain above 22 N/15 mm after filling at 35 kg load. Dart impact resistance is specified between 800 g and 1000 g for 100 μm film per ASTM D1709 Method A. REACH compliance applies, and no direct food-contact claim is made unless the specific additive package is tested under EU Regulation No 10/2011. SLL218 is not optimal for sack constructions requiring stiffness; if the sack body exceeds 130 μm gauge, blend addition of high-density polyethylene at 10–20 phr improves crease resistance but reduces low-temperature impact.

    What Limits Seal Strength After Ethylene Oxide Sterilisation in Laminated Sealant Webs?

    Sealant webs laminated to biaxially oriented polypropylene or polyester in dry food and medical device packaging are produced from SLL218 on cast film lines with a die gap of 0.7 mm to 0.9 mm, melt temperature from 240 °C to 260 °C, and chill roll temperature between 20 °C and 25 °C. Film thickness for the sealant layer is typically 20 μm to 30 μm. Formulation uses 100 parts SLL218, 5–15 phr LDPE or metallocene LLDPE to lower heat seal initiation temperature to 85 °C–95 °C, 0.5–1.5 phr silica antiblock masterbatch, and 0.2–0.5 phr erucamide slip masterbatch. Heat seal strength is measured by ASTM F88 with a 25 mm wide seal prepared at 120 °C, 1.4 bar seal bar pressure, and 0.5 s dwell. After ethylene oxide sterilisation at 38 °C and 60 % relative humidity, seal strength loss exceeding 15 % has been recorded when slip additive loading exceeds 0.4 phr; migrated erucamide forms a weak boundary layer at the seal interface. Medical packaging structures using SLL218 sealant webs therefore restrict the combined slip and antiblock package below 1.0 phr. The terminal laminate pouch is used for dry foods, powders, and medical devices requiring microbial barrier. Compliance must include FDA 21 CFR 177.1520 for olefin polymers, EU Regulation No 10/2011 with overall migration below 10 mg/dm², and ISO 11607-1 for medical packaging validation. The bio-based carbon fraction of SLL218 is verified by ASTM D6866-22 Method B; this value is not a substitute for performance compliance in sterile barrier systems.

    StandardRequirement
    FDA 21 CFR 177.1520Olefin polymer food contact; extraction maxima for hexane and xylene apply to the base resin and additive package
    EU Regulation No 10/2011Overall migration limit 10 mg/dm²; testing in simulant B and D2 for dry food and medical packaging depending on contact conditions
    ASTM D6866-22 Method BBiogenic carbon fraction from carbon-14 analysis for bio-based content verification
    ASTM F88/F88MSeal strength, specimen width 25 mm, test speed 300 mm/min
    ISO 11607-1Sterile barrier system performance, seal integrity and peelability after sterilisation

    Tear Anisotropy Management in Freezer-Grade Blown Film

    The anisotropy in dart impact and Elmendorf tear behaviour in SLL218 freezer film becomes significant when the bubble is collapsed at low frost line height or when blow-up ratio deviates from 2.5 to 3.0. On a three-layer blown line with die diameter 250 mm, die gap 1.8 mm, and melt temperature 195 °C to 220 °C, the layer distribution is set at 1/1/1 by output, with outer layers containing 0.3–0.6 phr of a low-temperature-stable slip/antiblock package. Formulation for the core layer is 90–95 wt% SLL218 plus 5–10 wt% LDPE; the LDPE component raises transverse-direction tear strength but reduces gloss. Film thickness for frozen vegetable and seafood bags is 40 μm to 70 μm, and the terminal pouch is run on vertical form-fill-seal machines at filling temperatures from -25 °C to -18 °C. Dart impact resistance measured at -20 °C according to ASTM D1709/A is used as a critical-to-quality value; a drop below 250 g at 50 μm thickness typically indicates excessive frost line height or insufficient LDPE. Elmendorf tear resistance per ASTM D1922 or ISO 6383-2 is used to quantify tear anisotropy; a machine-direction to transverse-direction ratio below 0.4 indicates excessive machine-direction orientation. The film is tested for low-temperature brittleness per ISO 974 or ASTM D746, and coefficient of friction is maintained between 0.15 and 0.30 per ASTM D1894 after 24 h conditioning at 23 °C. Direct food contact compliance is required; SLL218 must be used with an additive package and film structure meeting FDA 21 CFR 177.1520 and EU Regulation No 10/2011 overall migration below 10 mg/dm². Operational boundary: at chill roll or frost line conditions that produce excessive MD orientation, freezer bags exhibit zippered seal failure along the machine direction because oriented lamellae are susceptible to low-temperature crack propagation.

    On High-Output Rotary Ring Lines, Stretch Hood Draw-Down Demands Controlled Melt Strength

    Stretch hood lines operating at take-off speeds of 22 m/min to 28 m/min place a high draw demand on the film between the nip and the rotary ring. SLL218 is extruded on a three-layer blown line with die diameter 300 mm to 400 mm, die gap 2.0 mm to 2.5 mm, and blow-up ratio 3.0 to 3.5; melt temperature at the die is held at 190 °C to 215 °C. The structure uses 70–80 wt% SLL218 and 20–30 wt% LDPE to provide the necessary melt strength and transverse-direction elongation. Thickness is 50 μm to 150 μm, depending on pallet load weight and outdoor storage duration. The terminal film must stretch over 1200 mm by 1000 mm pallets and recover to secure the load. Published mechanical data for SLL218 in stretch hood constructions with specific rotary ring geometries is limited; converters typically set target values for dart impact at 600 g or above per ASTM D1709/A at 100 μm and tensile elongation at break above 500 % in both directions per ISO 527-3. Slippage of the film against the pallet cover is controlled by adding 0.3–0.6 phr of a high-molecular-weight silicone masterbatch to the inner layer, while the outer layer may contain 0.2–0.5 phr of a UV stabiliser for outdoor storage. Compliance is governed by the general industrial packaging requirements under REACH, and no direct food-contact claim is made for this construction unless the specific structure is brought into compliance with EU Regulation No 10/2011. A process failure mode observed on production equipment occurs when the blow-up ratio exceeds 3.5: the bubble becomes laterally unstable at high take-off speed and creates crescent-shaped thickness bands that reduce hoop recovery force.

    Free Quote

    Competitive Braskem Green PE SLL218 Blow Film Extrusion and Cast Film Extrusion Linear Low Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    Braskem Green PE SLL218 Blow Film Extrusion and Cast Film Extrusion Linear Low Density Polyethylene is a renewably sourced butene-comonomer linear low density polyethylene intended for monolayer and coextruded blown film and cast film conversion. The ethylene monomer originates in part from sugarcane ethanol, and the producer reports the renewable carbon fraction on the certificate of analysis under ASTM D6866-22. Representative values for the grade include a density of 0.918 g/cm³ when determined by ASTM D1505-18 and a melt mass-flow rate of 2.0 g/10 min at 190 °C with a 2.16 kg load using ASTM D1238-20 or ISO 1133-1:2022.

    The grade is positioned for flexible packaging applications where standard C4-LLDPE rheology is acceptable but a certified renewable-carbon content is required. Typical converted forms include form-fill-seal pouches, overwrap film, laminating substrate, collation shrink film, and general-purpose industrial packaging. SLL218 is not a high-pressure LDPE and is not a metallocene-catalyzed LLDPE; the linear backbone and butene short-chain branching produce lower melt tension than LDPE and typically lower clarity than metallocene LLDPE. These differences do not prevent its use in many blown film and cast film structures, but they require converter-specific processing discipline, particularly at high blow-up ratios and thin cast gauges below 15 µm.

    What distinguishes bio-based SLL218 from conventional C4-LLDPE film resins on a blown-film line?

    At equivalent density and melt mass-flow rate, SLL218 is designed to behave as a drop-in replacement for fossil C4-LLDPE in most monolayer and coextruded blown-film lines. The primary measurable distinction is the biogenic carbon content determined by ASTM D6866-22, rather than a fundamental change in melt viscosity or barrel pressure. However, short-chain branching distribution can differ sufficiently between product campaigns to shift seal initiation and hot-tack values. Converters should not transfer an existing fossil resin seal curve without confirmation. A seal curve is generated on the converted film by starting at 95 °C and increasing in 5 °C increments under constant dwell and jaw pressure.

    Compared to high-pressure LDPE, SLL218 has lower melt strength and reduced bubble stability at high frost line heights. A blown-film line that runs LDPE at a blow-up ratio above 3.0:1 may require internal bubble cooling or a narrower die gap with SLL218. Compared to metallocene-catalyzed LLDPE, the molecular weight distribution is generally broader, which reduces melt pressure and can improve bubble stability but also lowers notched tear and puncture resistance. Processing aid requirements should be determined by die shear rate; if sharkskin appears at die gaps below 0.8 mm, a fluoroelastomer processing aid at 200 ppm to 400 ppm is typically effective.

    On a production-scale monolayer blown-film line equipped with a 65 mm grooved-feed extruder, 30:1 L/D screw, and 250 mm die with a 1.8 mm die gap, stable bubble formation is normally reached with barrel temperatures of 170 °C to 190 °C and a die melt temperature of 200 °C to 215 °C. The blow-up ratio is maintained between 2.2:1 and 2.8:1, and the frost line is held at 5 to 7 die diameters. If the bubble oscillates, the first corrective action is to raise the lower barrel temperature slightly, reduce output by 5% to 10%, and lower the frost line. For cast-film extrusion, a 75 mm extruder with a 38:1 L/D screw and a 600 mm coat-hanger die can operate at a melt temperature of 240 °C to 260 °C. Chill roll temperature is set between 20 °C and 28 °C, and the air gap is kept between 10 cm and 15 cm. Films below 15 µm may require a vacuum box or a higher melt temperature to suppress draw resonance.

    No resin predrying is normally required when ambient relative humidity is below 60%. Above this threshold, surface moisture can create die-exit micro-bubbles and haze. Hoppers can be dried at 40 °C to 50 °C for 2 h to 4 h, or a dry-air hopper can be used. Long residence times above 10 min at melt temperature promote oxidation and gel formation; the adapter and die should be purged with a high-MFR LLDPE after line stops.

    Starting extrusion parameters for SLL218 in two film processes
    ProcessEquipment variableTypical starting range
    Blown filmDie gap1.8 mm to 2.0 mm
    Blown filmBlow-up ratio2.2:1 to 2.8:1
    Blown filmFrost line height5 to 7 die diameters
    Blown filmDie melt temperature200 °C to 215 °C
    Cast filmDie melt temperature240 °C to 260 °C
    Cast filmChill roll temperature20 °C to 28 °C
    Cast filmAir gap10 cm to 15 cm

    Rheological characterization on a capillary rheometer at 190 °C shows shear-thinning behaviour typical of linear low density polyethylene. Apparent viscosity decreases from roughly 1,200 Pa·s at 100 s⁻¹ to 150 Pa·s at 1,000 s⁻¹, but exact values should be taken from lot-specific curves. The critical shear rate for the onset of sharkskin depends on die gap and melt temperature; at 200 °C, die gaps below 0.8 mm can generate surface melt fracture unless a fluoroelastomer processing aid is present.

    Common blown-film defects include bubble oscillation, stalk sag, and melt fracture. Bubble oscillation is corrected by reducing air ring velocity or lowering the frost line; stalk sag indicates insufficient melt tension and can be addressed by reducing melt temperature or increasing die gap. Melt fracture appears as irregular transverse lines and is corrected by adding processing aid or increasing die temperature by 5 °C to 10 °C. In cast film, edge neck-in and draw resonance are controlled by reducing air gap, increasing melt temperature, or using a vacuum box. Thickness uniformity should be monitored by a capacitance gauge; deviations greater than ±5% in cast film influence seal performance and web handling.

    Tensile, tear, and dart impact thresholds in SLL218 monolayer films

    Film mechanical response is thickness- and orientation-dependent. For 25 µm monolayer blown film processed at a 2.5:1 blow-up ratio, machine-direction tensile strength is typically observed in the range of 30 MPa to 40 MPa and elongation at break in the range of 500% to 700% under ASTM D882-18. Elmendorf tear strength under ASTM D1922-21 generally falls between 120 g and 160 g in the cross direction for the same thickness. Dart impact determined by ASTM D1709-22 Method A on 25 µm film is commonly reported between 70 g and 100 g. These values are not guaranteed specifications; they are affected by blow-up ratio, frost line height, additive masterbatch, and testing laboratory humidity.

    Optical properties are also process-dependent. Cast film produced with a chill roll at 20 °C and an air gap of 10 cm can exhibit haze below 5% for 30 µm film under ASTM D1003-21, while blown film haze is typically higher. Gloss at 60° under ASTM D2457-21 is commonly 60 to 80 gloss units in cast film and 30 to 50 gloss units in blown film, depending on die design and frost line. Surface treatment by corona discharge at 38 mN/m to 42 mN/m is typical for printing and lamination; wetting tension is verified by ASTM D2578-23.

    In coextruded structures, SLL218 can serve as sealant layer, core layer, or external skin. A three-layer A/B/C film is commonly proportioned as 10% to 30% skin, 40% to 80% core, and 10% to 30% sealant. Regrind from edge trim and off-spec film can be reintroduced at 20% to 30% by mass in monolayer film. Higher regrind levels lower clarity and reduce dart impact. Contamination with polypropylene above 2% should be avoided because immiscible PP droplets produce haze and tear roughness.

    For extrusion lamination onto paper, board, or aluminium foil, SLL218 should be extruded through an air gap that is short enough to minimize oxidation but long enough to reduce neck-in. A typical air gap is 150 mm to 200 mm for coating width control. The melt curtain should be drawn down to a coating weight of 20 g/m² to 30 g/m² when the substrate allows. Adhesion is influenced by corona treatment, chill roll pressure, and substrate moisture. For foil lamination, a thin tie layer may be required if direct adhesion is below the target peel strength.

    For flexible food packaging, SLL218 is represented as complying with the olefin polymer provisions of FDA 21 CFR 177.1520, subject to finished-structure limitations and the additive formulation. European Union converters must perform migration testing on the final packaging under EU Regulation 10/2011 and its amendments; the resin certificate alone does not replace article-specific compliance. REACH Regulation 1907/2006 registration applies to the imported grade, and the material is not classified as dangerous under CLP Regulation 1272/2008. Restriction of hazardous substances is evaluated against Directive 2011/65/EU; maximum concentration values are 0.1% by weight in homogeneous material for lead, mercury, hexavalent chromium, PBB, and PBDE, and 0.01% for cadmium. The renewable carbon fraction is determined by ASTM D6866-22 and is reported as a percentage of total organic carbon; this value is not a biodegradability or compostability claim. SLL218 is not certified under EN 13432 and should not be specified for soil-degradable applications.

    Compliance and analytical references for SLL218
    AreaReference or methodCondition
    US food contactFDA 21 CFR 177.1520Olefin polymer provisions; article-specific limitations
    EU food contactEU Regulation 10/2011Migration testing on final packaging required
    Renewable carbonASTM D6866-22Biogenic carbon balance, lot-specific
    Hazardous substancesDirective 2011/65/EUPb, Hg, CrVI, PBB, PBDE 0.1%; Cd 0.01%
    ClassificationCLP Regulation 1272/2008Not classified as dangerous
    CompostabilityEN 13432Not certified for this grade

    Carbon footprint claims for SLL218 are generated through producer life-cycle assessments using ISO 14067 or the relevant greenhouse gas protocol; the documented reduction relative to fossil LLDPE is lot- and supply-chain-specific and should not be transferred without reviewing the product environmental profile. The bio-based carbon content of the polymer is not equal to the total renewable mass content because the mass balance and the chemical conversion of ethanol to ethylene are considered separately.

    When SLL218 replaces a fossil C4-LLDPE in cast-film, extrusion-lamination, and high-speed packaging lines

    Substitution is generally drop-in when the incumbent resin has equivalent density and melt flow rate. On cast-film lines, edge trim reincorporation should be held at 20% to 30% by mass to minimize gel accumulation in the feedblock and die lip. Extrusion lamination should operate at 290 °C to 315 °C to reduce melt viscosity for thin coatings; at these temperatures, the grade may produce more fume than high-pressure LDPE, which requires adequate extraction. In form-fill-seal packaging, seal initiation typically falls between 95 °C and 105 °C at 0.5 s dwell and 0.3 N/mm² jaw pressure, but the value must be confirmed by converter-generated seal curves. Hot-tack strength is generally adequate for vertical form-fill-seal lines running 40 to 60 packages/min. Above this range, or when sealing through heavy gussets, blending with a lower seal initiation metallocene LLDPE at 20% to 40% by mass may be required.

    Replacing high-pressure LDPE with SLL218 is not equivalent by mass. At 20% LDPE addition to SLL218, bubble stability improves but dart impact can decline relative to neat SLL218. In cast film, replacing metallocene LLDPE with SLL218 reduces clarity but often reduces melt pressure and die lip build-up. The appropriate replacement strategy is determined by the final packaging requirement: bio-based carbon content, sealing performance, optical clarity, or dart impact.

    The renewable-carbon benefit does not introduce a processing penalty in most lines, but contaminated or crosslinked scrap can create visible gel streaks and transverse-direction tear roughness. The operational boundary for cast-film edge trim reuse is approximately 30% by mass; above this threshold, gel agglomerates and die lip deposit can appear. Smooth-bore extruders should use feed zone temperatures below 170 °C to prevent early melt blockage. For high-output water-quenched cast film at line speeds above 300 m/min, published data for this specific configuration is limited, and converter trials are necessary to establish maximum stable line speed.

    Top