| HS Code | 815971 |
| Productname | Braskem Green PE SLH218 |
| Grade | SLH218 |
| Polymertype | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | 1-hexene |
| Renewablecarboncontent | 100% |
| Density | 0.918 g/cm³ |
| Meltflowrate | 2.3 g/10 min (190 °C/2.16 kg) |
| Meltflowratio | 28 |
| Meltingtemperature | 123 °C |
| Vicatsofteningtemperature | 100 °C |
| Tensilestrengthatyield | 11 MPa |
| Tensilestrengthatbreak | 25 MPa |
| Elongationatbreak | 700% |
| Flexuralmodulus | 260 MPa |
| Dartimpactstrength | 120 g |
| Haze | 12% |
| Gloss45degree | 80 |
| Coefficientoffriction | 0.2 |
| Processingmethod | Blow film extrusion and cast film extrusion |
| Recommendedmelttemperature | 180-210 °C |
As an accredited Braskem Green PE SLH218 Blow Film Extrusion and Cast Film Extrusion Linear Low Density Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaged in 25 kg moisture-barrier bags, palletized and stretch-wrapped, for safe transport of Braskem Green PE SLH218 resin pellets. |
| Container Loading (20′ FCL) | 20′ FCL container loaded with palletized 25 kg bags of Braskem Green PE SLH218 LLDPE for blow/cast film extrusion, strapped. |
| Shipping | Braskem Green PE SLH218 is a non-hazardous linear low-density polyethylene resin for blow/cast film extrusion. It ships in 25 kg bags or 1,000 kg octabins, palletized and stretch-wrapped, via standard truck, rail, or ocean container. No dangerous goods classification; keep dry, away from direct sunlight and heat. |
| Storage | Store Braskem Green PE SLH218 in a cool, dry, well-ventilated warehouse away from direct sunlight, heat, moisture, and ignition sources. Keep original packaging sealed and palletized. Avoid contamination, dust, and strong oxidizers. Maintain ambient temperatures; do not stack excessively. Protect from UV and follow first-in, first-out inventory practices. Ensure containers remain closed when not in use, and segregate from incompatible materials. |
| Shelf Life | Shelf life: 2 years from production date when stored in original packaging under dry, cool conditions, away from direct sunlight. |
Converting Braskem Green PE SLH218 into monolayer blown film for dry-food contact requires separation of renewable-carbon claims from the food-contact compliance dossier. The renewable carbon fraction is quantified by accelerator mass spectrometry under ASTM D6866 Method B, while food-contact status depends on the finished film meeting the extraction and migration limits defined in FDA 21 CFR 177.1520(c) and EU Regulation No 10/2011. In the U.S. market, the olefin polymer clearance applies when the resin constitutes the food-contact layer and is used under conditions of use appropriate for dry foods at room temperature; the conversion plant must also document that no recycled material in the food-contact layer violates the source control provisions of 21 CFR 174.5. Under the EU framework, the overall migration limit into food simulants must not exceed 10 mg/dm² or 60 mg/kg of food simulant, whichever is higher, when the finished article is tested under standardized time-temperature conditions. Specific migration limits for erucamide slip agents and other intentionally added substances are controlled by EU No 10/2011 Annex I, and the converter must retain supporting migration test reports for the final film structure rather than relying solely on neat resin certifications.
Formulation boundaries in dry-food monolayer bags are narrower than in industrial film because the additive package must remain within positive-list restrictions. The grade is typically run at 95–100 wt% neat in the food-contact layer; where horizontal form-fill-seal lines demand a lower coefficient of friction, converters add 0.3–1.0 wt% of a slip/antiblock concentrate based on erucamide and siliceous antiblock. A polymer processing aid may be used at 0.02–0.05 wt% only if its compositional substances are covered by EU No 10/2011 Annex I or equivalent national clearance. Dilution with 10–20 wt% LDPE is acceptable when the end-use requires more stable bubble geometry and a lower dart impact requirement; this shifts the seal initiation temperature downward by approximately 2–5°C per 10 wt% LDPE addition, which must be validated by differential scanning calorimetry and hot-tack testing on the actual film in the target thickness.
On a typical single-layer blown film line with a 250 mm die diameter and 2.0 mm die gap, the melt temperature is held between 190°C and 210°C, and the blow-up ratio is set between 2.2:1 and 2.8:1. Frost line height is maintained at 300–400 mm from the die face using a dual-lip air ring; internal bubble cooling is not required below 25 µm thickness but becomes advantageous at 40–50 µm to reduce blocking and increase output. The bubble is collapsed through a wooden or carbon-fiber collapsing frame, corona-treated to 38–42 mN/m before winding, and edge trim from the slitting section is re-ground and returned at 10–15 wt%. Higher regrind fractions can increase gel count and reduce seal strength at thin gauge, which is particularly limiting when the film is converted on high-speed vertical form-fill-seal machinery. Finished articles from this application include cereal liner bags, bread bags, rice pouches, sugar and salt sachets, and dry snack pillow packs.
| Regulation | Relevant clause or method | Boundary for this scenario |
|---|---|---|
| US FDA | 21 CFR 177.1520(c) | Food-contact layer for dry foods, room temperature, source control per 21 CFR 174.5 |
| EU | Regulation No 10/2011, Annex I/II | Overall migration 10 mg/dm² or 60 mg/kg; positive-list additives only |
| ASTM | ASTM D6866 Method B | Renewable carbon verification; not a food-contact permit |
| REACH | EC No 1907/2006 | SVHC and restriction compliance for EU marketing |
On high-output cast film lines, the quench temperature and air-gap distance govern the crystallinity development of SLH218-based stretch wrap more than the melt temperature alone. A chill roll temperature above 25°C increases haze and reduces transverse-direction elongation at break; a temperature below 18°C may create uneven quenching, especially at line speeds above 400 m/min. The cast stretch film application requires a melt flow rate at the high end of the LLDPE range to allow filling thin-gauge webs without excessive die pressure, and this grade is run with a target melt temperature of 240–260°C in the die zone. Compressor-side edge trim is re-cut and fed back through a pelletizer, with the recycled fraction maintained at 10–20 wt% to avoid accumulation of oxidised gel particles from repeated heat history. The industrial packaging converter tests cling and puncture performance with ASTM D5458 and ASTM D5748, while ASTM D4649 provides selection and use guidance for stretch wrap films.
Formulation admission boundaries differ from blown film food-contact systems. For a machine roll with a finished thickness of 20–23 µm, the cast stretch film formula typically contains 70–90 wt% SLH218, 10–30 wt% metallocene LLDPE or LDPE to adjust dart and puncture propagation, 0.5–2.0 wt% polyisobutylene cling agent, and 0.3–1.0 wt% anti-static concentrate. The cling agent is dosed in the core or skin layer depending on whether the line is a three-layer or five-layer cast coextruder; overdosing above 2.0 wt% causes roll telescoping and blocking, while underdosing below 0.5 wt% creates unwinding slip on pallet loads. Pull-off separation force between film layers is set against an internal converter specification derived from ASTM D5458, and the relationship between cling level and unwind speed is verified at the packaging line because warm warehouse conditions alter tack response more than ambient laboratory testing suggests.
Downstream production uses a flat-die cast film tower with a die width between 1800 mm and 3000 mm, an air gap of 8–12 cm, and a polished chilled roll with closed-loop temperature control. The melt curtain is pinned to the chill roll by an air knife or vacuum box; this maintains thickness variation below ±1.5% at high machine-direction output. Film thickness is measured continuously by beta-gauge sensors, and the signal is fed to the die bolt adjustment system. Pre-stretch rolls for hand-held application are produced at 12–18 µm, while machine-grade pallet wrap is produced at 20–30 µm. End products include hand stretch film rolls for pallet unitization, machine wrap for automatic rotary arm wrappers, and pre-stretched film for warehouses where dust and fog resistance are required. Compliance for industrial packaging falls under general REACH and packaging waste directive obligations, but not direct food-contact migration limits.
Low-temperature ductility of SLH218 in frozen vegetable and seafood packaging is governed by tie-chain density and the orientation state produced at the frost line, not by the renewable carbon content alone. At line speeds exceeding 250 m/min, residence time in the post-flame treatment zone is shortened, and the film enters the sealing jaw at a lower surface temperature unless active cooling is installed. This creates a risk of cold-seal voids in the longitudinal gusset region when the film is converted at -20°C storage temperatures. The recommended approach is to measure seal strength after conditioning per ASTM D618 at -20°C for 40 h, and to set the minimum hot-tack window using ASTM F1921 rather than relying on ambient seal curves. Evidence from high-speed packaging lines indicates that failure modes shift from seal-interface delamination at ambient temperature to film fracture adjacent to the seal at frozen storage temperatures, so the seal bar profile must be adjusted accordingly.
Formulation for frozen food packages uses 80–100 wt% SLH218 with 0–20 wt% LDPE to shift the seal initiation temperature lower; slip agent masterbatch is reduced to 0.1–0.3 wt% because excessive erucamide bloom can act as a wax-like contaminant at the seal interface and reduce cold-seal strength. An anti-fog concentrate at 0.5–1.0 wt% is included when the packaged product has high surface moisture; the concentrate must be selected from monomers with migration status in EU No 10/2011 Annex I and covered under FDA 21 CFR 177.1520 or applicable food-contact notifications. The direct food-contact compliance boundary is the same overall migration limit of 10 mg/dm², but the frozen-food condition is tested under simulated frozen storage rather than thermal abuse, and the converter must account for post-migration loss of low-molecular-weight additives during freeze-thaw cycling.
The blown film process for this scenario typically uses a coextrusion line with a die gap between 1.8 mm and 2.4 mm, melt temperature 195–215°C, and a blow-up ratio between 2.0:1 and 2.8:1. A higher frost line at 6–9 die diameters is maintained to shift impact resistance toward the machine direction, which is beneficial when downstream bag-making operates with a center-fold web. Internal bubble cooling is used to reach film thicknesses from 25 µm to 70 µm. Terminal products include frozen vegetable bags, IQF fruit pouches, frozen seafood packaging, and ice cream bags; these are produced on vertical form-fill-seal machines where the film must seal through minor product contamination at the seal area. The sealant layer in a coextruded structure is frequently the SLH218-rich skin, while the core contains the LDPE-rich blend for bubble stability. Published data for the exact low-temperature impact retention of this renewable grade is limited because most converters replace fossil-based LLDPE on the same line without re-optimizing the frost line, which can produce lot-to-lot differences in cold-durability performance.
Static charge accumulation on granulated polymer filling lines imposes a surface resistivity boundary on shipping-sack films that is separate from drop-impact performance. For heavy-duty form-fill-seal sacks made from SLH218-rich blown film, the surface resistivity is normally adjusted with an internal anti-static additive rather than topical post-treatment, because the sack must remain printable after corona treatment and must not accumulate carbon black dust. Drop-impact requirements are specified by the end customer using ASTM D5276 or an internal 1.5 m drop protocol; the film must also meet the tear-propagation and tensile criteria of ASTM D1922 and ASTM D882 after conditioning for 48 h at 23°C ±2°C and 50% ±10% relative humidity. In continuous filling trials, sacks produced with excessively high coefficient of friction can interrupt the FFS jaw cycle and generate heat-seal micro-holes, so the anti-static and slip additive levels are co-optimized rather than treated as independent variables.
The sack body formulation typically contains 70–85 wt% SLH218, 15–30 wt% LMDPE or LDPE, 2.0–3.0 wt% carbon black masterbatch when outdoor yard storage requires UV protection, and 0.02–0.08 wt% polymer processing aid. The carbon black loading must be kept below 3.0 wt% to avoid reducing tensile strength and weld-seam integrity; a loading at the lower end is acceptable for indoor warehousing. The structure is produced on a large-bubble blown film line with a die diameter of 350–450 mm, die gap 2.2–3.0 mm, melt temperature 190–215°C, and a blow-up ratio of 1.8:1–2.2:1. Gusseted collapsing frames create side gussets of 15–25% of the layflat width, and the film is corona-treated to 38–42 mN/m for flexographic print adhesion. Thickness per wall ranges from 80 µm to 130 µm, with the lower thickness used for small sacks and the upper thickness for export bags of petrochemical pellets and fertilizers.
Finished products from this segment include polymer resin sacks on automated FFS lines, fertilizer bags, salt export sacks, and industrial powder bags. The key operational boundary is the welding jaw temperature on the form-fill-seal machine; if the jaw temperature exceeds 160°C, the inner seal layer can stick to the release coating and cause micro-holes at the weld seam. Converters therefore validate the jaw temperature profile with a thermal camera and adjust line speed rather than increasing seal temperature unnecessarily. Compliance for these sacks is usually outside direct food-contact rules, but EU marketing requires REACH compliance and, when the sacks are used for dangerous solids, the packaging must satisfy the applicable national and international transport packaging requirements. The downgauging limit for a 25 kg petrochemical sack on a high-speed FFS line is typically around 70 µm per wall; below this thickness, the weld seam and drop-impact performance become too sensitive to normal filling-line abuse and batch-to-batch resin variation.
Anaerobic silage sealing imposes a different UV-stabiliser loading than general pallet stretch film because the film remains under tension across the full outdoor storing season. The mechanical requirement is not merely initial puncture resistance, but retention of elongation after prolonged weathering. In agricultural films, the relevant standard is EN 13207:2018, which sets requirements for thermoplastic silage films including thickness, width, mechanical properties, and resistance to tearing. Puncture resistance is conventionally evaluated by ASTM D5748, and tear propagation by ASTM D1922, with samples taken from both machine and transverse directions. However, the weathering boundary is often a customer specification rather than a harmonized standard; a common acceptance criterion is that the film must retain at least 50% of its initial elongation after 12 months of outdoor exposure in a temperate climate. Batch-to-batch variance in UV masterbatch dispersion can shift this retention threshold, so converters must verify masterbatch let-down uniformity by ash testing and tensile testing after accelerated weathering rather than relying only on supplier certificates.
The formulation for silage wrap is based on 80–95 wt% SLH218 with 5–20 wt% metallocene LLDPE to increase puncture resistance, 0.5–1.5 wt% UV stabilizer masterbatch containing HALS and a benzotriazole or benzophenone-type UV absorber, and 0.5–2.0 wt% polyisobutylene cling agent. The UV masterbatch dosing is increased to the upper limit when the film thickness is 20 µm and the bales are stored in southern exposure; overdosing above 1.5 wt% can reduce cling and increase roll noise during wrapping. The pigment package is normally white or green, with titanium dioxide loadings up to 2.0 wt%, because darker films absorb more heat and accelerate anaerobic fermentation but also risk black fungal growth at the bale surface. In multi-layer cast film structures, the UV stabilizer is concentrated in the core layer to reduce bloom on the cling skin layer.
Production is done on a cast film line with a multilayer die, melt temperature 235–255°C, chill roll temperature 15–22°C, air gap 6–10 cm, and a target film thickness of 20–30 µm. Edge trim is recycled at 10–20 wt%, but recycled UV-stabilized film should be limited because repeated heat histories consume the HALS activity and can produce a false sense of outdoor durability. Finished articles include round bale silage wrap in 750 mm width, square bale wrap, and silage clamp cover films where the same cast process is run at 30 µm or higher. The wrap is applied by round baler machines with a pre-stretch ratio of 60–70%; at stretching ratios above 70%, pin-hole defects can develop at the film edge, allowing oxygen ingress and spoilage of the silage. The puncture failure mode under repeated stretching is usually transverse-direction tear at the film edge rather than catastrophic machine-direction split, which differs from pallet stretch film and requires separate quality control on edge trim.
In retort-free lamination structures, the SLH218 sealant web is combined with biaxially oriented polyester or biaxially oriented polypropylene by solvent-free adhesive, and the downstream lamination process introduces an additional interlayer stress that is absent in monolayer film. The sealant layer is not exposed to direct retort temperatures, so the suitability assessment focuses on seal initiation temperature, interlayer bond strength, and the visual appearance of the renewable PE after lamination. Published data for this specific configuration is limited; converters generally validate seal initiation temperature with ASTM F1921 on the laminated film rather than relying on neat resin data. The interlayer bond strength is tested in a 90° or 180° peel mode following ASTM F904 after the adhesive has been cured for 48 h at 40°C. For food-contact laminates, the finished structure must comply with EU No 10/2011 Article 15 as a multi-layer food-contact material, and the food-contact layer itself must respect the overall migration limit of 10 mg/dm²; the non-food-contact outer layers may contain substances not listed for direct contact provided a functional barrier is demonstrated or migration is below the applicable limit.
The formulation boundary for the sealant web is 60–90 wt% SLH218, 10–40 wt% LDPE or mLLDPE to tune seal strength and interlayer bond performance, 0.1–0.5 wt% slip agent, and 0.05–0.15 wt% polymer processing aid. The upstream blown film process produces a sealant web of 30–50 µm thickness using a die gap of 2.0–2.4 mm, melt temperature 195–215°C, and a blow-up ratio of 2.0:1–2.5:1; the web is corona-treated to 40–44 mN/m before adhesive coating. Lamination is run at 150–250 m/min with a solvent-free polyurethane adhesive applied at 1.8–2.5 g/m², followed by re-winding and controlled curing. The terminal products include dry-food pouches, personal care refill pouches, household goods sachets, and non-food retail packaging where a renewable-carbon sealant layer provides differentiation without exposing the product to high retort temperatures. One operational limitation is the heat-seal jaw temperature: in laminated pouches, the seal dwell time is often shorter than in monolayer film, so the sealant layer must contain enough LDPE or mLLDPE to lower seal initiation temperature below the outer layer thermal distortion limit of 130–140°C. Failure to validate the sealant curve on the laminated structure, rather than on the free film, can result in channel leakers at the pouch corner seals.
Competitive Braskem Green PE SLH218 Blow Film Extrusion and Cast Film Extrusion Linear Low Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
The Braskem Green PE SLH218 grade is a linear low density polyethylene developed for blown film extrusion and cast film extrusion. The material is part of the producer's sugarcane ethanol–derived polyethylene portfolio and retains the molecular architecture of a conventional film-grade LLDPE. The grade is intended for thin-gauge flexible structures in which puncture resistance, tear propagation resistance, and low-temperature toughness determine package performance. The polymer is an addition copolymer of ethylene with a co-monomer that modifies the short-chain branching distribution; the producer's designation indicates a hexene-based LLDPE architecture. Unlike polylactic acid, starch-based materials, or polyhydroxyalkanoates, SLH218 is not biodegradable and is designed for conventional polyolefin recycling. It is supplied as free-flowing pellets and is used in stretch film, collation shrink film, industrial liners, lamination film, overwrap, and other monolayer or coextruded film structures. The renewable carbon content is the primary difference from petroleum-derived LLDPE grades, while conversion behavior remains within the same process window as conventional film-grade hexene LLDPE. The grade is synthesized from ethylene produced by dehydration of sugarcane ethanol. The melt flow rate places the resin in the medium-flow class for polyolefin film extrusion; the density places it in the low-density polyethylene range even though it is an LLDPE. The product can be processed on standard single-screw extruders without fluoropolymer die lip coatings or special corrosion-resistant screw materials.
The renewable carbon in SLH218 originates from ethanol produced by fermentation of sugarcane-derived sucrose. Ethanol is dehydrated to ethylene over an oxide catalyst at elevated temperature; the resulting bio-ethylene is polymerized using conventional coordination catalysts. The final resin is chemically indistinguishable from fossil LLDPE, but the fraction of bio-derived carbon can be quantified using ASTM D6866 or ISO 16620-2. Under ASTM D6866, the bio-based carbon fraction is determined by accelerator mass spectrometry measurement of the 14C isotope. Mass-balance certification under ISCC PLUS allows the producer to allocate renewable feedstock across the production chain without physical segregation at every unit operation. A certificate of analysis or sustainability certificate should be examined for the specific lot because the renewable carbon declaration can be allocated between shipments. The resin does not rely on water-soluble polymers, starch, or oxo-degradable additives for its renewable status. The dehydration of ethanol to ethylene can be carried out in adiabatic fixed-bed reactors; the crude ethylene is purified before polymerization. The resulting polymer is a non-polar hydrocarbon and does not contain oxygen in the polymer backbone, which differentiates it from polyesters and polycarbonates. The renewable carbon content is not a proxy for compostability. The grade remains a thermoplastic material that can be re-extruded and recycled in the same polyolefin streams as fossil LLDPE.
The release data sheet for SLH218 lists a nominal melt flow rate of 2.0 g/10 min when measured at 190 °C under a 2.16 kg load according to ISO 1133-1 or ASTM D1238. The nominal density is 0.916 g/cm³ as measured by ISO 1183-1 or ASTM D1505. These values place the grade in the low-melt-temperature, thin-gauge film extrusion class. The higher melt flow rate relative to a 1.0 g/10 min film LLDPE reduces motor load and screen-changer pressure on grooved-feed extruders but also lowers melt strength, which must be compensated in blown film by reduced blow-up ratios and careful frost line control. In cast film, the 2.0 g/10 min flow improves throughput across a narrow die gap and aids in gauge control at high line speeds. Because the resin is not hygroscopic, drying is not generally required below typical warehouse humidities. The crystalline melting point is typically in the range of 122 °C to 126 °C; this is a structural property determined by short-chain branching and not by the renewable origin. The thermal conductivity and specific heat of the melt follow the same range as fossil LLDPE, so existing screw cooling and barrel temperature profiles do not need to be re-engineered. Table 1 lists the property envelope reported for a 30 µm blown film under standard laboratory conditions; these are not lot-release limits and should not be substituted for the certificate of analysis.
| Property | Method | Reported typical value |
|---|---|---|
| Melt flow rate | ISO 1133-1 / ASTM D1238 | 2.0 g/10 min |
| Density | ISO 1183-1 / ASTM D1505 | 0.916 g/cm³ |
| Melting peak temperature, differential scanning calorimetry | ISO 11357-3 / ASTM D3418 | 124 °C |
| Tensile strength at break, machine direction | ISO 527-3 / ASTM D882 | 40 MPa |
| Tensile strength at break, transverse direction | ISO 527-3 / ASTM D882 | 32 MPa |
| Elongation at break, machine direction | ISO 527-3 / ASTM D882 | 650 % |
| Elongation at break, transverse direction | ISO 527-3 / ASTM D882 | 750 % |
| Dart impact F50, 30 µm film | ISO 7765-1 / ASTM D1709A | 80 g |
| Elmendorf tear, machine direction | ISO 6383-2 / ASTM D1922 | 40 g |
| Elmendorf tear, transverse direction | ISO 6383-2 / ASTM D1922 | 80 g |
| Haze, 30 µm film | ISO 14782 / ASTM D1003 | 8 % |
| Gloss at 60° | ISO 2813 / ASTM D2457 | 80 GU |
On production-scale blown film lines with die diameters from 50 mm to 150 mm, barrier screws with L/D ratios of 24:1 to 30:1, and Maddock mixing sections, SLH218 is typically processed at melt temperatures between 190 °C and 230 °C. The die gap is normally set from 0.8 mm to 1.2 mm for film gauges between 20 µm and 80 µm. Blow-up ratios above 2.5:1 can reduce bubble stability because the 2.0 g/10 min melt flow rate corresponds to lower extensional viscosity at the frost line; when ambient air temperature exceeds 28 °C, a lower frost line or a smaller bubble may be required to prevent slow oscillation. Field observations on grooved-feed extruders indicate that a screen pack of 80/80/120 mesh, a die temperature of 205 °C, and an internal bubble cooling system improve gauge uniformity in 25 µm film. A back-pressure of 100 bar to 250 bar at the screen changer is typical for a 90 mm extruder running at 250 kg/h; the exact value depends on screw speed and melt temperature. The resin has a melt elongation behavior that supports bubble diameters from small layflats to medium widths, but bubble instability has been observed on high-stalk configurations with very low frost line heights because the melt is faster-flowing than a fractional-melt LLDPE. The resin does not require pre-drying when stored below 60 % relative humidity; above that threshold, surface moisture can create micro-bubble defects in thin films, and a 70 °C dryer residence time of 2 h is normally sufficient. Gels are typically not observed at melt temperatures below 240 °C; sustained residence above 260 °C should be avoided because it can promote oxidation and crosslinking at the die lip.
In five-layer cast stretch film structures, SLH218 can serve in the cling or release layers if combined with appropriate tackifiers or slip additives. Since the resin is a non-polar LLDPE, cling properties are not inherent; they depend on low-molecular-weight polyisobutylene or sorbitan ester additives that migrate to the surface. The film's elongation and recovery behavior are governed by the LLDPE matrix, but the addition of tackifiers alters the coefficient of friction and may reduce optical transmittance. Machine direction orientation in blown film is influenced by the draw-down ratio, which is the ratio of die gap to final gauge divided by blow-up ratio. For a die gap of 1.0 mm and a final gauge of 25 µm, the resulting orientation can produce a measurable split in machine direction and transverse direction tensile properties. Converters should not rely solely on the resin's reported isotropic film properties; the anisotropic character of LLDPE films requires line-specific mapping.
In plants where films are printed or laminated immediately after extrusion, corona discharge treatment is often applied to raise the surface energy of the LLDPE. SLH218 responds to corona treatment similarly to fossil LLDPE, but the treatment level decays through additive migration; the surface energy should be verified at the winding station rather than immediately after the treater. The resin's antioxidant package can be modified by the processor if prolonged outdoor exposure is required, but such modifications should be validated for colour and gel formation.
Cast film extrusion of SLH218 is typically carried out at melt temperatures between 220 °C and 250 °C with a die gap from 0.4 mm to 0.6 mm. The higher melt flow rate allows the resin to pull down into thin gauges without exceeding the maximum screw speed on most production extruders. The air gap between die and chill roll is normally maintained between 5 cm and 15 cm; shorter air gaps reduce neck-in but can increase edge beading, while longer air gaps improve melt relaxation but may reduce film gloss. Chill roll temperatures are generally held between 20 °C and 30 °C. Cast film gauges from 12 µm to 50 µm are within the published processing window. At line speeds above 150 m/min, edge pinning systems are often required to prevent edge draw and uneven winding. For extruders with screw diameters below 60 mm, the 2.0 g/10 min melt flow rate may allow higher screw speeds without exceeding the maximum melt temperature. The use of a melt pump is optional but can reduce pressure pulsations in thin-gauge cast film. The resin's sensitivity to draw resonance is moderate; lowering the melt temperature or reducing the air gap can shift the onset of draw resonance to higher draw ratios. Static pinning systems using a corona discharge or vacuum box are necessary for line speeds above 100 m/min to stabilize the melt web against the chill roll. Published data for ultra-thin stretch film below 8 µm produced solely from SLH218 is limited, and converters should run pilot trials to confirm motor load, gauge profile, and puncture resistance before full-scale production.
Food-contact suitability is not established by the resin alone; the finished film must be assessed under the relevant jurisdiction. For polyolefins, compliance is commonly evaluated against FDA 21 CFR 177.1520 and Commission Regulation (EU) No 10/2011. The renewable carbon content does not alter migration behavior, but the final additive package, printing inks, and lamination layers contribute to the overall compliance assessment. For food contact assessment under Commission Regulation (EU) No 10/2011, the specific migration limits for ethylene and co-monomer residuals are generally not exceeded in fully polymerized polyolefins, but the final film must still meet overall migration limits. The resin's renewable origin does not exempt it from any substance restrictions under REACH Regulation (EC) No 1907/2006 or RoHS Directive 2011/65/EU. SLH218 should not be dry-blended with hygroscopic polar additives without vented extrusion because the resulting moisture uptake can produce surface defects. Peroxide masterbatches intended for viscosity breaking should be used only at addition levels specified by the masterbatch supplier after verification of the melt temperature profile; uncontrolled peroxide addition may generate macroscopic gels in the die lip and reduce film clarity. The grade is not intended for foam extrusion, rotational molding, or blow molding because the melt flow rate and molecular weight distribution are designed for film conversion.
The primary difference between SLH218 and a petroleum-derived hexene LLDPE with the same nominal melt flow rate and density is the origin of the carbon. Conversion behavior on blown and cast film lines is generally comparable because the molecular architecture is not altered by the renewable feedstock pathway. When compared with a lower-melt-flow Green PE film grade, SLH218 reduces melt pressure in high-output cast film operations but requires more attention to bubble stability in blown film. Compared with Braskem Green HDPE film grades, SLH218 produces films with lower secant modulus and higher elongation, making the material more suitable for stretch and cling applications than for rigid or high-stiffness packaging. Compared with a LLDPE grade containing slip and antiblock masterbatch, SLH218 in its neat form may require additive blending to meet coefficient of friction targets in high-speed packaging lines. The resin is often combined with a masterbatch containing erucamide or oleamide for slip, and silica or talc for antiblock; addition levels below 0.1 % can shift haze but are sometimes necessary for automated form-fill-seal equipment. Table 2 summarizes the principal comparative attributes.
| Attribute | SLH218 | Conventional fossil hexene LLDPE | Lower-MFR Green PE film grade |
|---|---|---|---|
| Renewable carbon certification | ASTM D6866 / ISCC PLUS | none | ASTM D6866 / ISCC PLUS |
| Nominal melt flow rate | 2.0 g/10 min | 2.0 g/10 min | 1.0 g/10 min |
| Nominal density | 0.916 g/cm³ | 0.916 g/cm³ | 0.918 g/cm³ |
| Primary film process | blown and cast | blown and cast | blown |
| Bubble stability in large blow-up ratios | lower | lower | higher |
| Relative motor load in cast film | reduced | reduced | higher |
Published data for ultra-thin cast film below 8 µm and thick blown film above 100 µm produced solely from SLH218 is limited; pilot trials are required to confirm gauge uniformity and bubble stability under specific line conditions.