| HS Code | 491888 |
| Productname | Borealis FG5190 |
| Manufacturer | Borealis |
| Polymertype | Linear Low Density Polyethylene (LLDPE) |
| Comonomer | Butene-1 |
| Density | 0.919 g/cm3 |
| Meltflowrate | 0.9 g/10 min (190 °C/2.16 kg) |
| Meltingtemperature | 123 °C |
| Vicatsofteningtemperature | 100 °C |
| Tensilemodulus | 250 MPa |
| Tensilestrengthatbreak | 35 MPa |
| Elongationatbreak | 700% |
| Dartdropimpact | 120 g |
| Elmendorftearstrengthmd | 100 N/mm |
| Elmendorftearstrengthtd | 120 N/mm |
| Haze | 10% |
| Gloss | 80 |
| Processingmethod | Blown film extrusion |
| Form | Pellets |
As an accredited Borealis FG5190 Linear Low Density Polyethylene factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Borealis FG5190 Linear Low Density Polyethylene is packaged in 25 kg polyethylene bags, typically supplied on pallets. |
| Container Loading (20′ FCL) | Borealis FG5190 LLDPE is loaded into 20′ FCL containers as palletized 25 kg bags, typically 20 metric tons per container. |
| Shipping | Borealis FG5190 Linear Low Density Polyethylene is a non-hazardous, solid pellet resin. Ship in clean, dry bulk trucks, containers, or 25 kg polyethylene bags. Protect from moisture, sunlight, contamination, and punctures. No temperature control is normally required. Store in a cool, dry, ventilated area. |
| Storage | Store Borealis FG5190 Linear Low Density Polyethylene in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, flames, and strong oxidizers. Keep bags or containers closed, off the floor, and protected from moisture, dust, and contamination. Avoid prolonged UV exposure. Use appropriate handling to prevent static buildup. Observe local regulations and supplier recommendations. |
| Shelf Life | Typically 24 months if stored unopened in original packaging, dry, cool, and protected from direct sunlight and moisture. |
In three-layer blown film lines producing 80–140 µm heavy-duty sack web for form-fill-seal conversion of petrochemical granulate, fertilizer blends, and cementitious dry mix, FG5190 is supplied to the outer skin layers at 60–80 wt% of the total polymer fraction, with 15–30 wt% long-chain-branched low-density polyethylene added for bubble stability and 5–10 wt% high-density polyethylene added for tensile modulus. The middle layer is run at 40–50 wt% in-line regrind and 50–60 wt% virgin LLDPE/LDPE blend to cap gel contamination from recycled edge trim. On a 65 mm grooved-feed extruder with a 30 L/D barrier screw and a 250 mm three-layer die at a blow-up ratio of 2.5:1 to 3.0:1, melt temperature is held between 195 °C and 210 °C at die entry. Die gap settings between 1.8 mm and 2.2 mm maintain stable bubble geometry; at die temperatures above 220 °C surface oxidation narrows the hot-tack window, and at throughput below 200 kg/h prolonged residence time increases measurable gel count in the seal layer.
Heat seal initiation temperature on the LLDPE-rich outer layer, measured at 0.5 N/mm² seal pressure and 0.5 s dwell on a 100 µm specimen, falls within the typical window of 105 °C to 115 °C. Hot-tack retention is evaluated according to ASTM F1921-18, dart impact according to ASTM D1709 Method A, Elmendorf tear according to ASTM D1922, tensile properties according to ISO 527-3:2018, and seal strength according to ASTM F88/F88M-21. Incoming resin lots are checked for melt mass-flow rate under ISO 1133-1:2022 at 190 °C, 2.16 kg, and density under ISO 1183-1:2019. The addition ratio for surface additives on the skin layer is typically 2.0–3.0 wt% silica-based antiblock masterbatch and 1.0–2.0 wt% erucamide slip masterbatch, while the middle layer excludes slip to preserve interlayer adhesion. A fluoroelastomer processing aid masterbatch may be added at 0.05–0.10 wt% to reduce die-lip deposits in long-campaign runs exceeding 72 h.
| Requirement | Standard or Regulation | Controlled Parameter |
|---|---|---|
| Melt mass-flow rate | ISO 1133-1:2022 | Lot-to-lot processing window |
| Density | ISO 1183-1:2019 | Material classification |
| Film tensile properties | ISO 527-3:2018 | Strength and elongation at break |
| Dart impact | ASTM D1709 Method A | Puncture resistance |
| Elmendorf tear | ASTM D1922 | Tear propagation resistance |
| Seal strength | ASTM F88/F88M-21 | Seal force to failure |
| Hot tack | ASTM F1921-18 | Seal strength during cooling |
| Food contact, where claimed | Regulation (EU) 10/2011, FDA 21 CFR 177.1520(c) 3.1a | Overall migration and compositional compliance |
Terminal article types include 25 kg heavy-duty sacks, FFS pillow sacks for petrochemical granulate, FIBC inner liners, and valve sacks for cementitious dry mix. Where direct food contact is claimed, compliance must be confirmed against the supplier lot-specific declaration under Regulation (EU) 10/2011 Annex I, Table 2 overall migration limit of 10 mg/dm², and under FDA 21 CFR 177.1520(c) 3.1a. For dangerous goods packaging, the converted sack is validated under the UN Model Regulations Chapter 6.5 drop and stacking tests. Pre-drying is not required at ambient storage below 80% RH; heavily compacted regrind exposed to condensation is dried at 70 °C for 4 h before reintroduction. Avoid HDPE addition above 15 wt% in the seal layer because low-temperature dart impact and hot-tack force deteriorate measurably on high-speed FFS conversion.
Agricultural greenhouse covers produced from FG5190 on three-layer blown film lines require a stabilisation package capable of surviving 150–200 µm film thickness for three to five seasons in Mediterranean and North African irradiation environments. The starting layer formulation is 70–80 wt% FG5190 in the outer layer, 15–25 wt% EVA with 14–18 wt% vinyl acetate content for infrared retention and low-temperature flexibility, 4–6 wt% HALS/nickel-quencher UV masterbatch, 1.0–1.5 wt% anti-drip masterbatch, and 0.05–0.10 wt% acid scavenger masterbatch. The middle layer carries 30–40 wt% regrind with 60–70 wt% virgin LLDPE/LDPE blend. Total EVA across the web is held below 25 wt% because higher vinyl acetate content reduces dart impact and tear propagation resistance under hooped greenhouse tunnel loading.Line configuration uses a 300 mm three-layer die, die gap 1.6–2.0 mm, blow-up ratio 2.5:1 to 3.2:1, melt temperature 185–200 °C, and frost line height 500–700 mm. After winding, the film is evaluated under EN 13206:2017 for agricultural covering films, with accelerated weathering according to ISO 4892-2:2013 at 340 nm and 0.51 W/(m²·nm). Tensile elongation at break of the aged outer layer is retained above 50% after 5,000 h in the release gate; published multi-season field data specific to FG5190 in every greenhouse locale is limited. Sulfur-containing pesticide sprays and halogenated fumigants accelerate HALS consumption and create brittle zones along ventilation folds. Alkaline washing agents and PVC-overspray contact cause premature anti-drip failure. Do not thermoform or repair with open-flame heat above 150 °C because the EVA phase degrades and the outer surface loses wetting tension below 38 dyn/cm. Terminal article types include greenhouse tunnel covers, side curtains, and white/black coextruded mulching films.
For oxygen-sensitive forage silage, a three-layer cast film line with a 2,500 mm slot die and 400 mm air gap chills the molten web at 18–22 °C and line speed 300–500 m/min to produce 20–25 µm film. FG5190 is run at 75–85 wt% of the total polymer fraction, with 10–20 wt% LDPE for melt stability, 4–6 wt% UV/HALS masterbatch, 2–4 wt% white titanium dioxide masterbatch to reduce ultraviolet transmission and raise albedo, and 1–2 wt% polyisobutylene tackifier masterbatch for wind-layer cohesion. The tackifier level is deliberately kept below 2 wt% to avoid telescoping on high-speed winding at 600 m/min.
Film performance is assessed under EN 14932:2018 for stretch thermoplastic silage bale wrap, with puncture strength measured according to ASTM D5748, tensile elongation according to ISO 527-3:2018, and oxygen transmission rate according to ISO 15105-2. Retained elongation after weathering under ISO 4892-2 is used for shelf-life validation. At pre-stretch ratios above 200% on automatic bale wrappers, local thinning below 8 µm is observed, causing elevated oxygen transmission and reduced resistance to stubble puncture. Do not blend with butene-rich LLDPE scrap from general stretch film sources above 20 wt% because cast web neck-in increases and unwind blocking force exceeds the clutch setting of automatic bale wrappers. Terminal article types include round bale silage wrap and high-density square bale wrap.
Unlike silage wrap, stretch hood conversion subjects the tubular film to a cold-stretch regime of 50–80% at application temperatures of 10–25 °C, so residual holding force after 30 min must remain above the packaging-system setpoint for pallet stabilization. The polymer blend is 80–90 wt% FG5190 and 10–20 wt% LDPE, with 0.5–1.0 wt% slip masterbatch and 0.3–0.8 wt% antiblock masterbatch. No tackifier is used; holding force is controlled by frost line height and film orientation. Shrink-to-stretch transition is avoided to keep the application temperature below the melting onset of the crystalline domains.On a 300 mm blown-film die with blow-up ratio 2.2:1 to 2.8:1, die gap 1.8–2.4 mm, melt temperature 190–205 °C, and frost line height 600–800 mm, the film is converted into 60–120 µm tubular webs. Elastic recovery and permanent deformation are evaluated under ASTM D5459-17, dart impact under ASTM D1709 Method A, and corona-treated surface wetting tension under ISO 8296 at 38 dyn/cm minimum for printability. At storage relative humidity above 85%, regrind from corona-treated film can generate gel specks; pre-drying at 70 °C for 4 h is applied to regrind only. Winder tension is kept below the blocking threshold of the slip package, and symmetrical air-ring cooling is required to prevent gauge banding during cold stretch. Terminal article types include pallet hoods for bagged food ingredients, construction materials, and beverage crates.
Adhesion-critical surface protection webs for stainless steel sheet, glass, and glossy plastic panels use FG5190 at 75–85 wt% as the base polymer, with 10–20 wt% LDPE for melt stability, 2–5 wt% tackifier masterbatch, 0.05–0.10 wt% antioxidant masterbatch, and 0.5–1.0 wt% antiblock masterbatch to control unwind force. Low gel content is critical because gel particles above 200 µm create visible defects on laminated protective surfaces. Cast film lines produce 30–60 µm webs at line speed up to 350 m/min, with chill roll temperature 15–22 °C and corona treatment to reach 38–42 dyn/cm. Residence time is limited through a 100/200 mesh screen pack to suppress gel formation from heat history.
Regulatory control for restricted substances is maintained under REACH Regulation (EC) No 1907/2006, Annex XVII, and RoHS Directive 2011/65/EU. Tensile properties are measured according to ISO 527-3:2018, and peel adhesion to steel is evaluated according to ASTM D3330/D3330M. Published data for FG5190-specific migration of tackifier under high-temperature lamination is limited; the adopted adhesive system must be characterized by the converter for storage above 40 °C. Avoid aromatic solvent-based printing inks before corona treatment because wetting tension drops below 38 dyn/cm and adhesion transfer increases during high-humidity storage. Terminal article types include surface protection films for stainless steel coil, glass sheet, and injection-moulded glossy plastic panels.
Competitive Borealis FG5190 Linear Low Density Polyethylene prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Borealis FG5190 Linear Low Density Polyethylene is positioned for blown-film applications that demand stiffness, impact resistance, and controlled seal performance. Supplier literature lists the grade with a nominal density of 0.919 g/cm³ when tested under ISO 1183-1:2019 and a nominal melt mass-flow rate of 0.9 g/10 min when tested under ISO 1133-1:2022 at 190 °C and 2.16 kg. The product falls between very-low-density sealant grades with densities below 0.915 g/cm³ and high-modulus HDPE film grades above 0.945 g/cm³; the density value predicts a secant modulus intermediate between those classes, while the melt-flow value is typical for blown-film extrusion. The grade is used in heavy-duty sacks, freezer packaging, lamination films, and form-fill-seal structures. Because the numerical values are typical and not specification limits, the current version of the Borealis product datasheet governs lot-specific values.
The grade’s position in the film-grade portfolio is defined by the melt index–density pairing. A melt mass-flow rate of 0.9 g/10 min is low enough to preserve melt strength on large blown-film dies but high enough to avoid excessive melt pressure on single-screw extruders. The density of 0.919 g/cm³ is selected to provide a seal-initiation temperature below high-density blown-film grades while retaining a room-temperature modulus above that of ultralow-density sealants. These values are measured on pellets or conditioned molded specimens; final film stiffness is always influenced by the degree of orientation and cooling rate imposed by the film line.
Film property development in FG5190 depends on the catalyst system and reactor configuration. The grade is associated with the Borstar multimodal polyethylene process, in which loop and gas-phase reactors operate in series. The resulting molecular weight distribution contains a high-molecular-weight component that carries a larger fraction of short-chain branching, while a lower-molecular-weight component contributes to melt flow. This separation reduces the melt-fracture and bubble-instability tendencies observed in monomodal LLDPE of the same melt index. Dynamic shear rheometry under ISO 6721-10 typically shows a shear-thinning index consistent with a broader distribution: complex viscosity at 0.1 rad/s and 190 °C may lie between 8 000 Pa·s and 12 000 Pa·s, while at 100 rad/s it falls to 300–500 Pa·s. Published data for the exact molecular weight distribution parameters of FG5190 is limited; the rheological values are therefore directional and must be confirmed on the production lot. The practical expression of this architecture is a stable stalk on high-stalk blown film lines and a wider processing window for bubble diameter.
Elongational behavior is part of the reason FG5190 is selected for high-stalk blown film. In high-stalk processes the melt is drawn over a longer distance before the frost line; materials lacking extensional strain hardening develop draw resonance and bubble breathing. The multimodal distribution in FG5190 supplies high-molecular-weight molecules that are oriented in the melt and increase elongational viscosity at large Hencky strain. The result is a stable bubble above a frost line height of 5–7 die diameters. This is particularly relevant when the film is run at blow-up ratios above 2.8 and with low-pressure air rings.
Conventional butene-based Ziegler-Natta LLDPE grades often exhibit a broad short-chain branch distribution in which the lower-molecular-weight fractions contain less comonomer, producing early melting fractions that affect optics and seal behavior. FG5190 differs because the multimodal design places the high-comonomer content preferentially in the high-molecular-weight tail, which increases tie-chain concentration and improves toughness without reducing stiffness. In blown film, this translates into a better balance of dart drop impact and secant modulus than a standard C4 LLDPE of the same 0.919 g/cm³ density and 0.9 g/10 min melt index. On a 200 mm spiral mandrel die with 1.2 mm die gap, the FG5190-type distribution typically maintains bubble diameter within ±2 mm during haul-off fluctuations, whereas conventional C4 grades may oscillate by ±5 mm under the same air-ring pressure. The trade-off is optical clarity: metallocene-catalysed hexene-based grades often produce haze below 7 % on 25 µm film, while FG5190 typically falls between 10 % and 15 % under ASTM D1003. The product is therefore selected when bubble stability and stiffness are more important than maximum clarity.
At the extruder, the shear-thinning behavior of FG5190 reduces motor load on single-flite grooved-feed extruders. A barrier screw with a spiral Maddock mixing element and an L/D of 30:1 allows a melt temperature of 195–215 °C without excessive shear heating. Lower melt temperatures increase die pressure; on a 160 mm die, die-inlet pressure commonly moves from 280 bar near 215 °C to 340 bar near 195 °C. Pressure is line-specific. Grooved-feed extruders with high torque can operate at screw speeds up to 90 min⁻¹, but output is usually limited by bubble stability rather than plasticating capacity. The die gap is normally kept at 1.2–1.8 mm; a gap below 1.0 mm raises shear stress and may introduce melt-temperature spikes, while a gap above 2.0 mm reduces orientation and yields lower machine-direction tensile strength. These values are processing guidelines, not specification limits.
Temperature profiles should be set in ascending order from the feed zone to the die. A typical profile on a 55 mm extruder is 170 °C, 180 °C, 190 °C, 200 °C, 205 °C from zone one to die head; the melt temperature measured at the die exit should be 200–210 °C. Screw cooling is generally not required after the first zone. Blow-up ratio is typically kept between 2.2 and 3.0; higher blow-up ratios improve transverse-direction tear but decrease machine-direction tear and can destabilize the bubble if the frost line is high. The frost line height is positioned at 5–7 die diameters for balanced orientation. On a 200 mm die, this corresponds to 1 000–1 400 mm above the die face. Internal bubble cooling is recommended when output exceeds 2.0 kg/h per cm of die circumference; without it, the frost line becomes unstable and gauge variation at ±5 % may degrade to ±9 %.
Gauge uniformity is influenced by air-ring pressure and die temperature uniformity. On a 200 mm die with a dual-lip air ring and internal bubble cooling, gauge variation can be held within ±4 % at haul-off speeds up to 30 m/min for 80 µm film. If frost line height is raised above 7 die diameters without increasing air quenching, the bubble becomes more sensitive to room turbulence, and gauge variation typically increases. Conversely, a frost line below 3 die diameters may produce high transverse-direction tear but lower machine-direction tensile strength and higher blocking tendency.
Heat-seal performance is evaluated with flat-jaw sealers and converted on vertical or horizontal form-fill-seal machines. Under ASTM F88/F88M, a 40 µm film can develop seal strength of 2–4 N/15 mm at 105 °C; the value rises to 8–12 N/15 mm at 130 °C and reaches a plateau before 140 °C. Hot-tack measurements on a rotary sealer require a dwell time of 0.5–1.0 s, jaw pressure of 0.3–0.5 MPa, and cooling time below 0.4 s. Published data for FG5190-specific hot-tack curves is limited, and the values depend on film gauge, slip additive level, and seal bar profile. On packaging lines running above 40 cycles/min, hot-tack is more critical than ultimate seal strength because the filled package weight creates peel forces during the cooling phase. The seal-initiation temperature of FG5190 is higher than a 0.915 g/cm³ very-low-density grade but lower than HDPE film; this intermediate value reduces the risk of blocking on frozen food lines while maintaining acceptable sealing time.
On vertical form-fill-seal machines, the film is often folded and sealed with heated jaws at 120–135 °C. The seal bar profile must be matched to the polymer seal curve; insufficient jaw parallelism produces channels in the seal area. Seal strength measured under ASTM F88/F88M is reported as force per 15 mm width; a value of 8–12 N/15 mm at 130 °C is generally acceptable for medium-weight frozen food packages. For heavy-duty sacks, lap seals are preferred because film thickness at 80–120 µm increases the required dwell time. The seal window narrows as line speed increases above 40 cycles/min, and hot-tack may become the limiting parameter rather than ultimate seal strength.
Mechanical property values for FG5190 are typically measured on controlled blown film produced with 1.2 mm die gap, 2.5 blow-up ratio, and 200 °C melt temperature. The table below is a representative profile assembled from public film-grade literature and is not a specification certificate. Some values are expressed as ranges because film gauge, frost line, and additive formulation influence the result.
| Property | Test method | Value |
|---|---|---|
| Density | ISO 1183-1:2019 | 0.919 g/cm³ |
| Melt mass-flow rate at 190 °C/2.16 kg | ISO 1133-1:2022 | 0.9 g/10 min |
| Melting temperature | ISO 11357-3 | 122–124 °C |
| Vicat softening temperature | ISO 306 | 96–100 °C |
| Secant modulus at 1 % strain, 40 µm film | ISO 527-3 | 200–240 MPa |
| Dart drop impact, 25 µm film | ASTM D1709 | 90–140 g |
| Elmendorf tear resistance, 40 µm film, MD/TD | ISO 6383-2 | 40–70 N/mm / 120–180 N/mm |
| Haze, 25 µm film | ASTM D1003 | 10–15 % |
Comparative selection among FG5190, conventional C4 LLDPE, and metallocene C6 LLDPE depends on the stiffness-optics-sealing triangle. A lower-density grade at 0.915 g/cm³ may reduce seal-initiation temperature by 5–8 °C but lowers secant modulus. A higher-density grade above 0.925 g/cm³ increases modulus beyond 250 MPa but narrows the seal window and increases blocking tendency. Metallocene grades can provide lower haze and improved hot-tack at equivalent density, but they often exhibit higher die pressure and lower bubble stability in high-stalk processes. FG5190 is therefore directed to lines where bubble stability and stiffness dominate, with optics being secondary. The choice between FG5190 and other grades is determined by conversion equipment and final package performance, not by density alone.
The table should not be used for competitive specification because film properties are highly dependent on gauge, blow-up ratio, frost line, and additive package. For design calculations, values should be taken from the current product datasheet or from a trial run on the target line. Published data for the FG5190-specific configuration in multilayer structures is limited; when the grade is buried behind a metallocene skin sealant, its contribution to seal initiation is not observed because the skin dominates the seal.
Slip and antiblock additives are often masterbatched at the converter. If the resin is supplied without high slip, the coefficient of friction may exceed 0.6 on 40 µm film; the addition of 1–2 % slip/antiblock masterbatch reduces it below 0.2 but can increase haze by 2–4 % and reduce hot-tack. These interactions must be tested on the production line because additive buildup on the die lip can alter the bubble and create stationary melt fractures.
In cast-film and lamination lines where high melt strength LDPE is often preferred, FG5190 can be used as a sealing layer but is not a direct replacement for LDPE extrusion-coating grades. The absence of long-chain branching reduces drawdown and increases neck-in on extrusion coating; converters should not select FG5190 for curtain coating of paperboard at line speeds above 150 m/min unless a high-pressure drop die and a short air gap are used. Published data for this specific configuration is limited. In coextruded cast film, the grade is more readily processed as a core or sealant layer, where the melt is supported by polypropylene or HDPE skins. Chill-roll temperatures of 15–25 °C are typical for surface clarity, but the optical performance remains below that of random-propylene copolymers.
At melt temperatures above 240 °C, thermo-oxidative degradation of LLDPE introduces gel particles that appear as hard specks in thin film. The die exit melt temperature should be kept below 240 °C, and preferably between 190 °C and 220 °C. In an extruder with an output below 0.8 kg/h per cm of die circumference, residence time may exceed 15 min, increasing degradation risk. During shutdown, the screw and die should be purged with a low-melt-index polyethylene or an LLDPE with higher stabilizer load. The product is not hygroscopic; pre-drying is not required for storage relative humidity below 60 %. Condensed surface moisture from cold-warehouse handling must be removed by drying at 40–50 °C for 2 h when sacks are opened in a heated converting room. Copper and copper-based alloys are incompatible in high-temperature melt contact because copper ions catalyze degradation; bronze screen packs and copper-containing heater surfaces should be isolated from the melt stream. Uncontrolled addition of high-acid additives should be avoided because acid-catalyzed degradation can discolor the film and reduce output consistency.
Food-contact status is not an intrinsic property of the raw polymer; it is a property of the final structure and the converting conditions. The polymer may be evaluated under EU Regulation (EC) No 1935/2004 and Commission Regulation (EU) No 10/2011, or under FDA 21 CFR 177.1520 for olefin polymers. Converters should request lot-specific food-contact statements and migration test reports under EN 1186 or equivalent methods. Laminating adhesives, printing inks, slip additives, and recycled content must be assessed separately because they are not covered by the base polymer certification. If the film is used in food-contact applications above 40 °C or with fatty foods, total migration and specific migration of additives may become the limiting regulatory parameters.