| HS Code | 965588 |
| Polymertype | Recycled Low Density Polyethylene (rLDPE) |
| Recycledcontent | 100% recycled LDPE |
| Form | Pellets |
| Color | Natural |
| Density | 0.921 g/cm³ |
| Meltflowrate | 0.70 g/10 min at 190°C/2.16 kg |
| Tensilemodulus | 200 MPa |
| Tensilestressatyield | 10 MPa |
| Tensilestrainatbreak | 500% |
| Meltingtemperature | 110 °C |
| Vicatsofteningtemperature | 90 °C |
| Shoredhardness | 48 |
| Waterabsorption | 0.01% |
As an accredited Borealis Borcycle™ NAV101L Recycled LDPE factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Borealis Borcycle™ NAV101L Recycled LDPE is packaged in 25 kg polyethylene bags, palletized and stretch-wrapped for secure shipping. |
| Container Loading (20′ FCL) | 20′ FCL container loading: Borealis Borcycle™ NAV101L Recycled LDPE in 25 kg bags, palletized, kept dry, clean, and securely stowed. |
| Shipping | Borealis Borcycle™ NAV101L Recycled LDPE is typically shipped as non-hazardous, free-flowing pellets in sealed bags or octabins, palletized and stretch-wrapped. Transport in clean, dry, covered vehicles at ambient temperature. Protect from moisture, direct sunlight, heat, and contamination. Not regulated for transport. Store in original packaging; avoid prolonged hot storage. |
| Storage | Store Borealis Borcycle™ NAV101L Recycled LDPE in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, and open flames. Keep containers tightly closed when not in use. Avoid contact with strong oxidizers and incompatible chemicals. Prevent pellet spillage and clean up promptly to reduce slipping hazards. Protect material from moisture, contamination, and excessive temperatures. Follow local regulations. |
| Shelf Life | Shelf life is approximately 24 months when stored in original packaging, dry, cool, away from direct sunlight and heat. |
Blown film lines processing Borealis Borcycle™ NAV101L as a secondary feedstock for non-food heavy-duty packaging require differentiated barrel profiling and screen-pack monitoring because recyclate gel bodies and low-molecular-weight fractions alter bubble stability at low frost-line settings. The material is let down at 20–40 wt% into virgin LDPE with an ISO 1133-1:2022 melt flow rate of 0.7–1.0 g/10 min at 190°C/2.16 kg. Extrusion is carried out on a single-screw blown film line with a barrier screw of 25:1–30:1 L/D, a Maddock mixing section, feed throat temperature 35–45°C, barrel zones from 150°C to 175°C, and melt temperature 160–185°C. Die diameter is held at 250–350 mm, die gap at 1.0–1.5 mm, blow-up ratio at 2.0:1–2.5:1, and frost line height at 350–500 mm. Screen-pack differential pressure is recorded at start-up and after 4 h; a delta P rise above 2.0 MPa indicates gel accumulation requiring screen change. Compliance for non-food packaging requires EU 94/62/EC Annex II heavy-metal sum limits of 100 mg/kg and REACH Article 33 candidate list screening below 0.1% w/w per article. Tensile properties are tested under ASTM D882-12, dart impact under ASTM D1709-16a Method A, and gel dispersion under ISO 18553:2002. Terminal products include refuse sacks, industrial liners, pallet shrouds, and heavy-duty shipping sacks.
In extrusion coating of non-food paper and board, Borealis Borcycle™ NAV101L is introduced at 10–30 wt% into virgin LDPE to limit draw-down and neck-in defects. The coating line operates with a coat-hanger slot die, air gap 150–250 mm, chill roll temperature 12–18°C, die melt temperature 260–300°C, and line speed 80–150 m/min. Because gel particles from recycled LDPE disrupt the adhesion interface at low melt temperature and preferentially oxidize at extended air gaps, the air gap is not increased beyond 250 mm without trial confirmation. Adhesion to kraft paper is evaluated under ASTM D903-98(2017), coating weight is controlled gravimetrically under ISO 536:2019, and neck-in is measured at the die edge with a tolerance of 25–60 mm. Compliance for imported non-food laminates requires EU 94/62/EC Annex II heavy-metal limits of 100 mg/kg and REACH Article 33 screening below 0.1% w/w. Published data for this specific configuration is limited above 300°C; oxidative surface degradation may reduce peel strength before visible melt fracture appears. Terminal products include industrial paper sacks, protective interleaving, non-food pouch laminates, and release paper coatings.
Blending Borealis Borcycle™ NAV101L into injection moulding compounds at 15–50 wt% is constrained by thin-wall flow-length reduction and short-shot variability caused by the higher melt elasticity of post-consumer LDPE. The moulding cell is configured with a general-purpose screw of 20:1–22:1 L/D, clamp force 800–1,600 kN, melt temperature 160–200°C, mould temperature 15–30°C, injection pressure 50–80 MPa, and holding pressure 30–50 MPa. When ambient relative humidity exceeds 60%, the recyclate is pre-dried at 60–70°C for 2 h to limit surface splay. Shot weight variation is monitored within ±0.5% on production-scale machines to detect fill instability. Compliance for industrial non-food articles is verified under REACH Annex XVII restricted substances and RoHS Directive 2011/65/EU Annex II when overmoulded electrical or electronic accessories are produced: lead threshold 1,000 mg/kg, cadmium threshold 100 mg/kg, mercury threshold 1,000 mg/kg, hexavalent chromium threshold 1,000 mg/kg in homogeneous materials. Tensile properties are determined under ASTM D638-14, and notched Izod impact under ASTM D256-10. Terminal products include storage totes, edge protectors, damping pads, material-handling trays, and snap-fit industrial housings.
The following compliance matrix consolidates the regulatory standard designations applicable to each downstream conversion route.
| Conversion route | Standard | Test method or clause | Threshold / control |
| Blown film | EU 94/62/EC | Annex II | Sum Pb/Cd/Hg/CrVI ≤ 100 mg/kg |
| Extrusion coating | REACH | Article 33 | SVHC ≤ 0.1% w/w |
| Injection moulding | RoHS 2011/65/EU | Annex II | Pb ≤ 1,000 mg/kg; Cd ≤ 100 mg/kg |
| Rotational moulding | ASTM D1998-15 | Material property requirements | Design stress and wall thickness |
| Drip irrigation pipe | ISO 9261:2004 | Clause 5 | Dimensional stability |
| Extrusion blow moulding | EU 94/62/EC / REACH | Annex II / Article 33 | Heavy metals ≤ 100 mg/kg; SVHC ≤ 0.1% w/w |
Rotational moulding conversions of Borealis Borcycle™ NAV101L are restricted to 10–25 wt% let-down into virgin LDPE rotational moulding grades because higher recycled content reduces environmental stress crack resistance and low-temperature impact performance. The biaxial rotational moulding machine is operated at primary-to-secondary axis speed ratios between 4:1 and 6:1, oven temperature 250–280°C, total cycle time 20–30 min, and wall thickness 4–8 mm. Cooling is controlled at 2–3°C/min through forced air before water mist to prevent warpage and internal porosity. Oversized recyclate particles above 1,000 µm increase pinhole risk in thin-wall sections and are screened prior to powder blending. Compliance for non-food storage tanks is evaluated under REACH and ASTM D1998-15, with environmental stress crack resistance tested per ASTM D1693-15 Condition B and low-temperature impact under ASTM D1998-15 referenced methods. Published data for this specific grade in rotational moulding is limited; a full ESCR regression should be generated on the production tool before fixed formulation release. Terminal products include secondary containment basins, agricultural sprayer tanks, non-potable water storage tanks, and chemical dosing day tanks.
In low-pressure agricultural drip laterals, Borealis Borcycle™ NAV101L is let down at 15–30 wt% with virgin LDPE or LLDPE; above this range the hoop strength of the lateral and the dimensional accuracy of emitter orifices show unacceptable batch-to-batch variance. The pipe extrusion line uses a grooved-feed extruder of 25:1–28:1 L/D, a die and sizing mandrel for 12–20 mm outer diameter, vacuum calibration at -0.02 MPa to -0.05 MPa, melt temperature 170–190°C, and line speed 10–30 m/min. Die-entry melt pressure is monitored at 10–18 MPa to ensure dimensional consistency, and emitter orifice diameter variance is maintained below 2% coefficient of variation. Compliance for agricultural micro-irrigation components is assessed against ISO 9261:2004 for emitters and emitting pipe and REACH Title VIII restrictions. Hydrostatic pressure resistance is measured per ISO 1167-1:2006, and tensile properties per ISO 527-2:2012. Terminal products include drip irrigation laterals, micro-tubing, soaker hose, and low-pressure agricultural distribution tubing.
Extrusion blow moulding of non-food technical containers from Borealis Borcycle™ NAV101L is run at 25–50 wt% let-down into virgin LDPE blow moulding grades; the upper limit is set by parison melt strength and bottle wall thickness distribution rather than melt index alone. Single-station accumulator blow moulding equipment with clamp force 150–300 kN, die head 40–80 mm, and parison swell ratio 1.4:1–1.7:1 operates at melt temperature 165–185°C, mould temperature 5–20°C, and cycle time 35–60 s. Parison pinch weld and tail flash regrind can be reintroduced at 10–15 wt% as an internal reclaim stream, provided the combined recycled stream does not exceed the specified NAV101L let-down. Compliance for non-food technical containers requires EU 94/62/EC Annex II heavy-metal limits of 100 mg/kg and REACH Article 33 screening below 0.1% w/w. Environmental stress crack resistance is determined per ASTM D1693-15 Condition B, and drop impact for filled containers per ASTM D2463-15. Terminal products include non-food jerrycans, dosing tanks, technical hollow parts, and industrial fluid reservoirs. Hazardous goods certification is not claimed without additional UN packaging approvals.
Competitive Borealis Borcycle™ NAV101L Recycled LDPE prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Borealis Borcycle™ NAV101L is a mechanically recycled low-density polyethylene (rLDPE) grade supplied as a pelletised compound for non-food-contact film and sheet conversion. The grade identifier NAV101L denotes a controlled post-consumer polyolefin stream that is melt-filtered and compounded to a narrower melt-flow and density window than unsorted post-consumer LDPE regrind. Published datasheet values include a melt flow rate of 0.7 g/10 min at 190°C/2.16 kg under ISO 1133-1:2022 and a nominal density of 0.921 g/cm³ under ISO 1183-1:2019. Lot-specific certificates of analysis report melt-flow variation, gel count, colour coordinates, and filter-pressure behaviour. Because the feed stream derives from post-consumer packaging, direct food-contact use is not assumed; any food-contact structure must be evaluated under Regulation (EU) 2022/1616 or behind a functional barrier with migration testing under Regulation (EU) 10/2011.
The principal difference is specification stability rather than chemical identity. A generic post-consumer LDPE regrind entering the plant can vary from 0.3 g/10 min to 3.0 g/10 min in melt flow rate and may carry paper labels, aluminium remnants, and high-density polyethylene fractions; NAV101L is sold with a defined melt-flow band and specified contaminant limits. Against virgin LDPE of the same nominal density, NAV101L shows higher gel content, lower clarity, and a wider smoke point, so it is not interchangeable in high-gloss or high-clarity grades. Compared with chemically recycled Borcycle C materials or virgin LDPE, NAV101L retains the thermal history and oxidation products of the original polymer, which lowers long-term thermal-oxidative stability unless an antioxidant package is adjusted. Batch-to-batch colour variation is typically wider than virgin material because pigment feedstocks are not fully separated; converters using 1–3 wt% white masterbatch should validate opacity and colour coordinates at the start of each silo.
On a conventional blown-film line using a 60 mm single-screw extruder with a 25–30 L/D barrier screw, the recycled grade should be processed with a continuous melt filter of 100–150 μm and a screen pack of 60/100/60 mesh as a minimum. Melt pressure at the breaker plate commonly runs 15–25% higher than an equivalent virgin LDPE with the same melt index due to residual particulate matter. A die gap of 1.6–2.0 mm and blow-up ratio of 2.0:1–3.0:1 provide sufficient melt strength for films from 40 μm to 150 μm. Start-up temperature should be 175°C in the feed zone, ramping to 195–205°C in the metering zone; operation above 210°C increases volatilisation of residual odour compounds and promotes additional gel formation from degraded paper labels and adhesives.
Mechanical test results obtained from 50 μm blown-film samples are not identical to virgin LDPE; published data for this specific grade configuration is limited, and converters should rely on the certificate of analysis for tensile elongation and dart-drop values. When tested according to ISO 527-3:2018, the material generally exhibits lower tensile strength and elongation at break than prime LDPE because of chain branching and gel-induced stress concentrations. Tear resistance measured under ISO 6383-2:1983 is sensitive to film gauge, cooling air temperature, and frost-line height. For heavy-duty shipping sacks, the critical output is not the resin value alone but the converted film’s drop-impact resistance after side gusseting and bottom sealing; a standard dart-drop test under ASTM D1709 method A or B is appropriate for incoming inspection, with acceptance thresholds set per film gauge and end-use.
For cast extrusion and extrusion coating, the absence of biaxial orientation means melt strength is less limiting, but odour and gel content become more visible at coating weights below 25 g/m². A closed-loop melt temperature of 285–310°C is typically required for stable web neck-in, but this temperature window conflicts with the grade’s tendency to generate additional oxidation products; therefore, operation at the lower end is preferred, with a cast-roll temperature of 18–25°C and a matte finish roll to mask gel defects.
A recurring processing constraint with post-consumer recyclate is not melt-flow variability but contaminant-induced screen blockage. In production-scale trials on a 75 mm single-screw extruder with 28 L/D and a continuous slide-plate screen changer, start-up differential pressure across a 120 μm screen was observed to rise from 90–110 bar to above 140 bar within 4–6 h when running NAV101L at 380 kg/h. The pressure rise corresponds to filtration cake accumulation of oxidised gel particles, paper fibrids, and unmelts; if the operator increases screw speed to compensate for pressure drop, melt temperature rises and accelerates further gel formation. A filtration mesh of 100 μm is the minimum for film below 60 μm; 150 μm is adequate for heavy-gauge construction sheet where visual gel defects are less critical. The gel-count specification should define the maximum number of gels larger than 200 μm per square metre, with typical incoming inspection thresholds of 30–60 gels/m² for industrial film and 10–20 gels/m² for printing-grade surface layers. These values are operational targets, not guaranteed resin properties, because gel distribution is lot-dependent.
Odour control remains a measurable boundary in applications where the film is stored in enclosed spaces or used in retail packaging. Neutralisation is achieved by adding 1–2 wt% of a zeolite-based odour scavenger or a low-volatile antioxidant package; the addition level must be verified after a 48 h oven test at 60°C using an odour panel based on VDA 270 or equivalent in-house sensory methods. Surface treatment for printing requires a minimum surface tension of 38 mN/m to 42 mN/m when tested with inks according to ISO 8296:2003; recycled LDPE may require higher corona output or a longer dwell time because low-molecular-weight oxidation products migrate to the surface and reduce treatment stability.
Melt temperature selection for NAV101L should not be copied from virgin LDPE of the same melt index. The temperature profile should be flat to slightly reverse: 170°C in the feed throat, 180–190°C in the compression zone, and 190–200°C in the metering and die zones. A flat profile reduces the residence time at high temperature and limits the formation of carbonyl species from oxidised post-consumer gel particles. Die-gap settings should be 1.8–2.2 mm for blown film and 0.6–0.8 mm for cast film; a wider die gap lowers shear heating at the die lip and reduces die-lip build-up. The frost-line height should be held stable at 6–10 times the die diameter; an unstable frost line indicates output fluctuation, screen blockage, or incoming moisture. Pre-drying is not required for dry pellet, but surface condensation from cold silo storage can be removed with 60–70°C dehumidified-air drying for 2–4 h when relative humidity exceeds 60%.
| Process variable | Blown film | Cast film / coating |
|---|---|---|
| Melt temperature, °C | 190–200 | 285–310 |
| Die gap, mm | 1.8–2.2 | 0.6–0.8 |
| Blow-up ratio / draw ratio | 2.0:1–3.0:1 | — |
| Melt filtration, μm | 100–150 | 100–150 |
| Pre-drying | 60–70°C, 2–4 h if wet | 60–70°C, 2–4 h if wet |
Blending with 10–30 wt% virgin LDPE is common when the final film must pass a printing or lamination surface. The addition of virgin LDPE raises the average melt-flow stability and dilutes gel particles, but the blend’s property response is non-linear; at addition levels above 30 wt%, the recycled grade no longer provides the intended PCR content for sustainability certification. At 5–10 wt% addition of a low-molecular-weight LDPE carrier, the die-pressure fluctuation is reduced, but tensile strength and dart-drop impact can decline by 8–15% relative to the unblended recyclate. Pigment concentrates for recycled LDPE should be based on LDPE or EVA carriers with a melt-flow rate above 20 g/10 min to ensure dispersion at the lower melt temperatures used with NAV101L; high-viscosity masterbatches produce visible specks. Screw speed should be held within 70–85% of the extruder’s maximum torque, with gate and die pressures monitored continuously because the melt filter is the first component to indicate lot-to-lot contamination.
Regulatory status is a function of the recycling process route and the intended Member State market. Because NAV101L is mechanically recycled from post-consumer packaging, it is not automatically authorised for direct food-contact use; converters must confirm that the recycling process is listed under Regulation (EU) 2022/1616 or that the recycled layer is separated by a functional barrier. General product safety documentation should demonstrate compliance with REACH Regulation (EC) No 1907/2006, including any candidate-list substances, and with RoHS Directive 2011/65/EU for restricted heavy metals in electrical or electronic packaging applications. For agricultural silage film, the relevant performance characteristic is not food-contact status but UV stabilisation and oxygen permeability; a minimum UV-stabiliser package of 0.3–0.5 wt% HALS, based on resin weight, is typically required to survive 12–24 months outdoor exposure. Construction film is governed by national specifying bodies and may require a minimum thickness, tear resistance, and flame retardancy; no single European standard covers all construction film, so declarations are made against the nearest product standard such as EN 13206 for covering films or EN 13361 for geomembranes.
| Regulation / standard | Designation | Application relevance |
|---|---|---|
| REACH | Regulation (EC) No 1907/2006 | Substance registration and candidate-list screening |
| RoHS | Directive 2011/65/EU | Restricted heavy metals when used in EEE packaging |
| Food-contact plastics | Regulation (EU) 10/2011 | Migration testing if barrier or food-contact status is claimed |
| Recycled plastic food contact | Regulation (EU) 2022/1616 | Process authorisation for direct food-contact recycled polymer |
| Melt flow rate | ISO 1133-1:2022 | Incoming lot control |
| Density | ISO 1183-1:2019 | Incoming lot control |
| Surface tension | ISO 8296:2003 | Printing and lamination readiness |
For collation shrink and light agricultural tunnel film, the grade performs best when the converter specifies the widest gel tolerance and uses a printing design with high ink coverage or a surface matte finish. A blown-film structure of 80–120 μm with 2:1 blow-up ratio is less sensitive to gel aesthetics than a 25 μm high-clarity wrap. In a multi-layer coextrusion, NAV101L should be placed in the core or the back layer of a three-layer structure, with virgin LDPE skins of 10–15% total thickness to stabilise surface gloss and seal initiation. This arrangement retains recycled content while preventing gel and surface oxidation from defining the sealing and printing behaviour.