Bestrade Group Kaladex Pen Film 2000 Dumfries

Bestrade Group Kaladex® PEN Film 2000 (Dumfries)

    • Product Name: Bestrade Group Kaladex® PEN Film 2000 (Dumfries)
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 404230
    Material Polyethylene naphthalate (PEN)
    Orientation Biaxially oriented
    Density 1.36 g/cm³
    Thickness Range 12–500 µm
    Melting Point 265 °C
    Glass Transition Temperature 120 °C
    Tensile Strength 200 MPa
    Tensile Modulus 5 GPa
    Elongation At Break 100%
    Heat Shrinkage 1.5% at 150 °C
    Dielectric Constant 3.2 at 1 kHz
    Dissipation Factor 0.002 at 1 kHz
    Water Absorption 0.4%
    Haze 1.5%
    Refractive Index 1.65

    As an accredited Bestrade Group Kaladex® PEN Film 2000 (Dumfries) factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing Supplied as 200 kg rolls, individually wrapped in protective film and packed in sturdy, labelled cardboard cartons for safe transport.
    Container Loading (20′ FCL) 20′ FCL container loading for Bestrade Group Kaladex® PEN Film 2000 (Dumfries): securely packed, stowed, and restrained for safe transport.
    Shipping Bestrade Group Kaladex® PEN Film 2000 (Dumfries) is shipped as non-hazardous polymeric film in rolls on pallets under ambient, dry conditions. Protect from moisture, heat, UV, and mechanical damage. No special dangerous-goods classification; follow local transport and handling regulations.
    Storage Store Bestrade Group Kaladex® PEN Film 2000 in a cool, dry, clean, well-ventilated area at ambient temperature, away from direct sunlight, UV light, heat, ignition sources and moisture. Keep in original sealed packaging, upright, and protect from dust, solvents, sharp objects and physical damage. Maintain stable humidity, avoid contamination, do not stack heavy items, and follow manufacturer and local storage/shelf-life instructions.
    Shelf Life Shelf life is typically indefinite when stored in original packaging in a cool, dry, well-ventilated place away from direct sunlight.
    Free Quote

    Competitive Bestrade Group Kaladex® PEN Film 2000 (Dumfries) prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    Bestrade Group Kaladex® PEN Film 2000 (Dumfries) is a biaxially oriented polyethylene naphthalate film supplied as a converter-grade web. The 2000 designation functions as a base-film grade identifier; in converter practice it is commonly interpreted as a nominal 50 µm thickness, although certificate-of-analysis values govern any lot-specific downstream decision. The Dumfries qualifier serves as a traceability marker for the Bestrade Group supply node and does not modify the polymer backbone or surface treatment. The product is based on poly(ethylene 2,6-naphthalate), formed by melt-phase esterification of ethylene glycol and 2,6-naphthalenedicarboxylic acid, followed by biaxial stretching and heat-setting. The naphthalate ring system increases chain stiffness relative to polyethylene terephthalate and raises the glass transition temperature while reducing segmental mobility.

    Physical property expectations for biaxially oriented PEN film are governed by backbone rigidity and heat-set conditions. Published data for this specific Dumfries-supplied configuration is limited; representative values from public PEN film literature place density at 1.36 g/cm³ under ISO 1183-1, glass transition temperature near 120 °C by ISO 11357-2, and machine-direction tensile modulus at approximately 5.5 GPa under ASTM D882. These figures are comparative envelopes rather than product specifications. Slit widths and roll lengths are order-specific; no universal standard width should be inferred from the grade designation.

    Within the PEN film family, the 2000 grade differs from thinner gauges principally in bending stiffness, which scales with the third power of thickness. A 50 µm web is approximately eight times stiffer in flexural rigidity than a 25 µm web at equivalent modulus. That stiffness reduces handling wrinkles during adhesive lamination but increases minimum bend radius in flexible circuit coverlay applications. Drying after aqueous processing also requires longer residence because the moisture diffusion path length doubles relative to 25 µm. Thickness uniformity should be verified by ISO 4593 or the supplier certificate rather than inferred from roll weight.

    How Does the Naphthalate Backbone Alter Barrier Response in 2000-Grade PEN Film?

    Gas transport in polyethylene naphthalate differs from polyethylene terephthalate because the fused naphthalene ring restricts free-volume segmental oscillations. In practical terms, oxygen permeability is reduced by roughly a factor of 5 at equal thickness when compared with PET at 23 °C and 0 % RH using ASTM D3985. Water vapour transmission is also lower, although the differential narrows at high humidity because surface hydrogen-bonding effects become more influential. For a 50 µm web, published PEN barrier data cluster near 8 cm³/(m²·day·atm) for oxygen and 2.5 g/(m²·day) for water vapour at 38 °C and 90 % RH under ASTM F1249. These values support applications where retort flavour retention or oxygen-sensitive electronic components are specified, but they are not unique to the Dumfries supply stream.

    The activation energy for oxygen permeation in biaxially oriented PEN is higher than in PET; as temperature increases from 23 °C to 50 °C, oxygen transmission rate rises less steeply. This reduces the barrier penalty during warm warehouse storage. However, the barrier advantage can be degraded by thickness variation or microvoids introduced during overstretching. Film thickness uniformity should therefore be measured by ISO 4593 or equivalent optical gauge, and not inferred from average roll weight or total length.

    When evaluated against conventional PET films, the 2000-grade PEN product occupies a higher thermal class. The differential in glass transition temperature is approximately 42 °C above PET. The practical effect appears as reduced thermal shrinkage after 30 min at 150 °C under ASTM D1204, with public PEN values near 0.1 % compared with 0.3–0.5 % for common heat-set PET grades. That dimensional stability reduces registration drift in multi-up flexible circuit printing and in selective adhesive coating operations.

    PropertyTest StandardRepresentative PEN 2000Representative PET
    DensityISO 1183-11.36 g/cm³1.40 g/cm³
    Glass transition temperature, DSCISO 11357-2120 °C78 °C
    Tensile strength at break, MDASTM D882280 MPa250 MPa
    Tensile modulus, MDASTM D8825.5 GPa4.0 GPa
    Elongation at break, MDASTM D88280 %120 %
    Thermal shrinkage, 150 °C, 30 min, MDASTM D12040.1 %0.3–0.5 %
    Oxygen transmission rate, 50 µm, 23 °C, 0 % RHASTM D39858 cm³/(m²·day·atm)40 cm³/(m²·day·atm)
    Water vapour transmission rate, 50 µm, 38 °C, 90 % RHASTM F12492.5 g/(m²·day)5.0 g/(m²·day)
    Dielectric strengthIEC 60243-1220 kV/mm200 kV/mm
    Dielectric constant, 1 kHzIEC 602503.23.3

    Published data for this specific product configuration is limited; the table is a comparative envelope drawn from public PEN and PET film literature and should not substitute for certificate-of-analysis values. Lot-to-lot variation in heat-setting, surface treatment, and slitting at the Dumfries node can shift dimensional and adhesion values by several percentage points. Converter qualification should therefore include retained samples from each incoming lot and not rely solely on generic polymer-class data.

    Processing Above the Critical Shrinkage Threshold Introduces Registration Drift in Multi-Up Printing

    The higher glass transition temperature of PEN does not eliminate constrained-shrinkage sensitivity; it moves the onset upward. Converter experience in roll-to-roll lamination with tension control of ±1.5 N per 10 cm web width indicates that uncontrolled zone temperatures above 170 °C can still produce cumulative machine-direction shrinkage sufficient to shift flexible printed circuit registration by more than 0.2 mm across a 500 mm repeat. The critical processing threshold lies not at the glass transition but at the heat-set temperature of the film. For high-yield multi-up work, web tension should be profiled so that the film enters each thermal zone under a maximum of 1.0 % yield strain. Drying after aqueous washing should follow lot-specific supplier profiles rather than generic PET settings. A common converter benchmark is 120 °C for 10 min, but that value is not a substitute for process qualification.

    On a multi-zone drying tunnel, the film should be supported by low-tension rollers with a maximum unsupported span of 1.5 m between idlers. If the film passes through a coating head with a gap set below 1.5 times the web thickness, surface defects can propagate into subsequent die-cutting stations. These are field observations from roll-to-roll converting rather than standard specifications. Solder float resistance is commonly assessed by immersion in molten solder at 260 °C for 10 s according to IPC-TM-650 2.4.13. PEN 2000 films typically show no blistering or delamination under these conditions if the web has been dried to a moisture content below 0.1 %. PET films are marginal at this temperature because their glass transition is much lower. This differential is a primary selection criterion for lead-free assembly.

    Applications for this film grade include flexible flat heating elements, membrane touch switch spacers, high-temperature wire and cable wrap, and flexible printed circuit coverlay or base substrate where lead-free solder float resistance is required. In each case the film is used because its dimensional stability at 180 °C to 200 °C exceeds PET and its cost is lower than polyimide. For membrane touch switch spacers, the surface can be hard-coated or primer-treated; adhesion values above 10 N/25 mm are achievable with acrylic adhesives after corona treatment, but adhesion should be verified by ASTM D3330. The film also absorbs UV below 380 nm more strongly than PET because of the naphthalene chromophore. This characteristic is advantageous for UV-blocking labels but complicates UV-cured adhesive lamination because through-film curing is attenuated. Radiant energy and lamp focus should be validated with a dosimeter; belt speed may need to be reduced by 20–30 % compared with PET processing under the same lamp array.

    When 2000-Grade PEN Film Replaces Polyimide in Flexible Substrate Laminates

    Polyimide replacement is justified only for operating temperatures below the PEN thermal class. Continuous-use exposure above 160 °C in air will reduce tensile elongation faster than polyimide; published PEN ageing data show embrittlement after several hundred hours at 180 °C, whereas polyimide survives longer. Electrical insulation properties, however, are often comparable at lower voltages. PEN film typically exhibits dielectric strength near 220 kV/mm under IEC 60243-1 and a dielectric constant near 3.2 at 1 kHz under IEC 60250. It also offers better moisture resistance than polyimide, which can be important in condensation-prone automotive sensor circuits. The replacement is therefore appropriate when the service environment is below 150 °C continuous and when humidity resistance outweighs extreme thermal endurance.

    Electrical testing on biaxially oriented PEN film should be carried out after conditioning at 23 ± 2 °C and 50 ± 5 % RH according to ISO 291. Dielectric breakdown is strongly influenced by thickness homogeneity; converters should measure at a minimum of 5 points across the web to capture edge effects. Surface roughness below 0.05 µm Ra is typical for optical-grade precursor film, but the Dumfries stock may be supplied with a non-treated or corona-treated surface depending on the purchase specification. In flat flexible heating elements, the film acts as a dielectric carrier for etched foil or carbon-printed resistors. The service temperature typically remains below 120 °C, making PEN a lower-cost alternative to polyimide. Thermal cycling between -40 °C and 120 °C for 1000 cycles has been reported in public PEN literature without significant delamination when the adhesive system is matched to the film surface. The film should not be used as a standalone insulation layer in direct contact with live parts above the voltage rating of the printed circuit; design verification should follow IEC 60664-1 clearance and creepage requirements.

    Oligomer Deposition and Solvent Attack at the Adhesive Interface

    Cyclic oligomers in PEN are less prone to migrate than PET oligomers because the stiffer chain lowers diffusion coefficients; nevertheless, prolonged exposure to solvent-based lamination can extract low-molecular-weight species. Methyl ethyl ketone and toluene blends used in flexible circuit adhesives can swell the film surface if line speed is too low or drying capacity is insufficient. The film should not be combined with unreacted isocyanate or amine-based adhesion promoters without verifying that the substrate surface pH remains below 8, because alkaline conditions accelerate ester hydrolysis at elevated humidity. Chlorinated solvents such as methylene chloride are generally compatible for cleaning but should be evaporated below the heat-set temperature to avoid surface haze. Published data for the specific interaction of the Dumfries-supplied film with aggressive solvent blends is limited; therefore, a lamination trial with 500 m of production web is recommended before full qualification.

    Hydrolysis resistance is superior to PET because the naphthalate ester is sterically shielded, but hydrolytic degradation still occurs in retort above 121 °C over multiple cycles. Long-term contact with strongly alkaline solutions above pH 9 at temperatures above 60 °C should be avoided. Acidic conditions below pH 3 can also reduce molecular weight at elevated temperature. No established test standard covers all laminate configurations; suppliers should be consulted for extraction data and lot-specific chemical resistance. The film should be stored in the original moisture-barrier packaging at 10–30 °C and below 60 % RH. If the packaging has been opened and the web has been exposed above 70 % RH for more than 24 h, pre-drying at 150 °C for 4 h with a dew point of -40 °C or lower may be required before thermal processing. In high-humidity storage, the surface treatment may decay through reorientation of polar groups; surface energy should be re-verified by dyne solutions or contact angle measurement after prolonged storage. The product is not intended for continuous-use service above 160 °C without application-specific ageing validation.

    Top