| HS Code | 298544 |
| Polymer Type | PBT |
| Glass Fiber Content | 15% |
| Molding Shrinkage Percent | 0.3-0.8 |
| Ul94 Flammability | HB |
| Volume Resistivity Ohm Cm | 1E16 |
As an accredited BASF Ultradur® PBT+GF15% B4521 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Supplied in 25 kg moisture-proof bags and palletized, protecting the glass-fiber-reinforced PBT resin during storage and transport. |
| Container Loading (20′ FCL) | BASF Ultradur® PBT+GF15% B4521 loaded in a 20′ FCL container, palletized in 25 kg bags, dry and secured for transport. |
| Shipping | BASF Ultradur® PBT+GF15% B4521 is typically shipped as non-hazardous thermoplastic pellets in moisture-barrier bags, 25 kg sacks, or octabins on pallets. Transport at ambient temperature; keep dry and protected from direct sunlight, moisture, punctures, and prolonged heat. Follow the SDS and local transport regulations. |
| Storage | Store BASF Ultradur® PBT+GF15% B4521 in a cool, dry, well-ventilated area away from direct sunlight, heat sources, moisture, and incompatible materials. Keep containers sealed, labeled, and free from contamination or physical damage. Use original packaging and follow first-in/first-out stock rotation. Avoid dust generation and prolonged outdoor exposure; dry pellets as specified before processing. |
| Shelf Life | When stored dry and in unopened packaging at recommended conditions, BASF Ultradur PBT+GF15% B4521 typically has a 12-month shelf life. |
Competitive BASF Ultradur® PBT+GF15% B4521 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
BASF Ultradur® PBT+GF15% B4521 is a polybutylene terephthalate injection-moulding compound reinforced with a nominal 15% by weight of short E-glass fibre. Under ISO 1043-1 the material is designated PBT-GF15. The glass-fibre content is controlled by ash-content methods according to ISO 3451-1; because the density of E-glass is close to 2.54 g/cm³ and the PBT matrix density is near 1.31 g/cm³, the nominal weight fraction corresponds to roughly 9% by volume. BASF technical literature reports the compound density at 23 °C as 1.41 g/cm³ when determined to ISO 1183-1. Pellets are supplied for injection moulding; the matrix is a polybutylene terephthalate homopolymer with an ester linkage that is sensitive to hydrolysis in the melt phase. Moisture uptake in the solid state is moderate compared with polyamide, but melt-phase water controls molecular weight retention and therefore the final mechanical response.
The product is used in automotive connector bodies, relay bases, switch housings, sensor brackets, and small structural housings for power tools. The selection logic is usually a compromise between the low flow resistance of unfilled PBT and the higher stiffness but higher density and warpage of PBT-GF30. Published data for this specific configuration is limited in peer-reviewed literature; therefore tool-specific filling and warpage studies are required. The material is not designed for continuous exposure to hot water above 60 °C or to strong alkaline media at elevated temperature, because hydrolysis of the ester linkage would proceed at an unacceptable rate.
Before processing, B4521 must be dried to a residual moisture content below 0.04% as measured by Karl Fischer titration or ISO 15512. Drying in a dehumidifying desiccant dryer with a dew point not higher than -30 °C at 120 °C for 4 h is sufficient for sealed, undamaged bags. If the pellets have been exposed to relative humidity above 60% for more than 24 h, the drying time is extended to 6 h. A hopper dryer without desiccant cannot reliably achieve this level in humid plant air. When wet melt enters the barrel, hydrolytic chain scission lowers molecular weight; the first visible processing symptoms are surface streaks, followed by a drop in Charpy notched impact strength to ISO 179-1/1eA and an increase in melt volume-flow rate to ISO 1133-1. On a production-scale injection-moulding machine, batch-to-batch variability in moisture is therefore more likely to cause property drift than variability in glass content.
| Variable | Recommended band | Measurement basis |
|---|---|---|
| Residual moisture | 0.02–0.04% | Karl Fischer or ISO 15512 |
| Melt temperature | 250–270 °C | Barrel set points, rear to nozzle |
| Mould temperature | 60–100 °C | Cavity surface before injection |
| Cushion | 2–5 mm | Screw position at hold switchover |
| Residence time | 3–8 min | Calculated from shot weight and barrel capacity |
| Back pressure | 5–15 bar hydraulic | Machine gauge; actual melt pressure depends on cylinder diameter |
Injection-moulding screws for this grade should have a compression ratio of 2.0–2.5 and a length-to-diameter ratio of 20–25. General-purpose polyolefin screws with short feed sections can generate glass-fibre accumulation at the check ring and unacceptable shot-to-shot variation. Screw pull-back after plasticising should be limited to 2–5 mm; larger decompression draws air into the melt film and produces silver streaks. Mould venting at the perimeter of the cavity should be cut to 0.015–0.030 mm because PBT has a low melt viscosity and deeper vents encourage flash. On hot-runner systems, open-pipe geometries with uniform thermal profiling are preferred. Valve-gate systems can be used, but fibre accumulation at the poppet seat becomes a known failure mode when the gate seat clearance is below 0.03 mm. Mould temperature below 60 °C tends to produce a faster surface freeze and higher gloss but less complete crystallinity; subsequent annealing at 120 °C can produce dimensional changes up to 0.1% in unfavourable flow orientations.
The grade is compounded on twin-screw equipment with high-shear dispersion sections; the initial chopped strand length of 3–4.5 mm is reduced to an average fibre length in the moulded part of 200–400 μm. Because fibre length affects tensile strength more than stiffness, lot-to-lot variation in fibre length distribution should be monitored by incineration and image analysis when tight mechanical specifications apply. The addition of regrind can further reduce average fibre length; in production, regrind addition above 25% commonly reduces Charpy notched impact by 10%–20% relative to virgin pellets.
Flowability of B4521 is specified by the melt volume-flow rate under ISO 1133-1 at 250 °C and 2.16 kg. BASF technical data for the grade report an MVR in the 17–24 cm³/10 min range. The MVR is a single-point index for lot release and does not capture the shear-thinning behaviour of a glass-filled melt. For thin-wall connector bodies with wall thickness of 0.8–1.2 mm, filling is governed by gate diameter, venting, injection velocity, and cavity pressure. Spiral-flow tests on equivalent PBT-GF15 compounds at 250 °C and 100 MPa injection pressure typically give flow lengths of 200–300 mm in a 1 mm spiral, but published data for this specific configuration is limited and cannot replace tool-specific filling simulation. Raising melt temperature within the 250–270 °C band improves knit-line strength but accelerates molecular weight loss; the upper temperature limit is therefore set by degradation kinetics rather than by short-shot risk.
At shear rates encountered in injection moulding, the apparent viscosity of glass-filled PBT decreases strongly with increasing shear. Capillary rheometry data on equivalent PBT-GF15 grades show an apparent viscosity at 250 °C of approximately 150–250 Pa·s at 100 s⁻¹ and 40–70 Pa·s at 1,000 s⁻¹. The highest fibre orientation occurs in high-shear gate regions and in the frozen skin layer; the core contains a more random orientation distribution. As a result, tensile modulus in the flow direction is typically 1.6–2.2 times the transverse modulus in moulded specimens. For this reason, flexural modulus measured on a 4 mm plaque is not a reliable predictor of bending stiffness in a 1 mm wall. Mould shrinkage to ISO 294-4 for PBT-GF15 is typically 0.5–0.7% parallel to flow and 1.0–1.5% transverse to flow; the difference is a primary source of warpage in flat parts with uneven rib distributions.
Tensile modulus to ISO 527-1/-2 for B4521 is reported in the range 4,500–6,000 MPa, with tensile stress at break near 90 MPa and tensile strain at break between 2.0% and 3.0%. Flexural modulus to ISO 178 is slightly different, typically 4,600–5,400 MPa, because flexural loading imposes a strain gradient and samples the oriented skin layer. Charpy notched impact strength to ISO 179-1/1eA at 23 °C is in the range 4.0–5.5 kJ/m²; the value remains above approximately 3 kJ/m² at -30 °C because the polyester matrix does not exhibit the pronounced low-temperature ductile–brittle transition seen in unreinforced polyamide. Heat deflection temperature under 1.8 MPa to ISO 75-1/-2 is approximately 185–195 °C, compared with 50–60 °C for unfilled PBT. The glass transition remains near 45–60 °C; the fibre network maintains load-bearing capacity well above the glass transition until the crystalline phase melts around 220–225 °C.
Within the Ultradur portfolio, B4521 is positioned between an unfilled PBT such as B4520 and a 30% glass-fibre PBT such as B4300 G6. At 15% glass, the density penalty over unfilled PBT is approximately 0.10 g/cm³, whereas PBT-GF30 adds roughly 0.22 g/cm³. The 15% grade provides about twice the tensile modulus of unfilled PBT and roughly half the additional stiffness of a 30% glass-fibre grade. In moulded parts with ribs, bosses, and holes, the 15% material shows less differential shrinkage between flow and cross-flow directions than PBT-GF30; anisotropic shrinkage ratios for PBT-GF30 can exceed 2.5, while PBT-GF15 typically remains below 2.0. The trade-off is lower creep resistance and lower notched impact than a 30% glass-fibre grade. The following indicative envelope, derived from standard injection-moulded specimen data, provides a systematic comparison:
| Property | Test method | Unfilled PBT | PBT-GF15 | PBT-GF30 |
|---|---|---|---|---|
| Density | ISO 1183-1 | 1.30–1.31 g/cm³ | 1.39–1.43 g/cm³ | 1.51–1.56 g/cm³ |
| Tensile modulus | ISO 527-1/-2 | 2,400–2,700 MPa | 4,500–6,000 MPa | 9,000–11,000 MPa |
| HDT/A at 1.8 MPa | ISO 75-1/-2 | 50–60 °C | 185–195 °C | 200–210 °C |
| Charpy notched 23 °C | ISO 179-1/1eA | 3–5 kJ/m² | 4–5.5 kJ/m² | 6–9 kJ/m² |
The values are not single-lot certificate data and reflect fibre orientation, moisture conditioning, and test-specimen geometry. The Charpy comparison demonstrates that impact strength does not scale linearly with glass content; the 15% grade is closer to unfilled PBT than to PBT-GF30 in notched impact, while its modulus lies in the upper half of the range between unfilled PBT and PBT-GF30. For snap-fit and press-fit connector geometries, the B4521 grade is often preferred over PBT-GF30 when lower surface roughness and lower post-mould warpage matter more than maximum stiffness; if creep under continuous spring load is dominant, PBT-GF30 is usually substituted.
In automotive under-hood connector housings, B4521 is typically processed with a melt temperature of 260 °C and a mould temperature of 80 °C to control post-mould warpage across pin arrays. The clamp force requirement is often estimated at 0.5–0.7 kN per cm² of projected area; for a multi-cavity tool with a projected area of 400 cm², a machine with at least 2,000 kN clamp force is selected. Peak cavity pressures in such tools are frequently 40–70 MPa. Flash at the parting line indicates that cavity pressure has exceeded the clamping pressure at the tool periphery. In production, shunt faults in connector bodies after moulding are usually traceable to thermal degradation creating carbonised particles that block pin holes, rather than to glass-content variation; drying and residence-time control therefore dominate lot acceptance.
For electrical insulation components, the comparative tracking index to IEC 60112 for PBT-GF15 is typically in the 400–600 V range, depending on pigment and sizing. Surface resistivity to IEC 60093 is usually above 1013 Ω on dry moulded surfaces; after high humidity or water immersion, surface leakage must be managed through creepage and clearance distances to IEC 60664-1 rather than by relying on surface resistivity alone. The grade is normally classified HB to UL 94 at 1.5 mm and greater; for V-2 or V-0 requirements, a flame-retardant PBT or a PBT/PA blend is typically substituted. Continuous-use temperature is limited by thermo-oxidative embrittlement; standard PBT grades in UL 746B long-term heat ageing often receive relative temperature indices in the 120–140 °C range, but the specific RTI for B4521 must be obtained from the current UL yellow card.
Melt-phase degradation of PBT is accelerated by oxygen; hydrogen abstraction from the butylene segment produces hydroperoxides that decompose to carbonyl species. Above 270 °C, visible discolouration from yellow to brown can occur within 5 min in a standard injection-moulding barrel. Degradation is routinely monitored by MVR increase and carboxyl end-group concentration. Shot size should be at least 40% of barrel capacity; lower shot fractions extend the residence time of a portion of the melt and increase variability. In gas-assist injection moulding or long hot-runner channels, local hold-up volumes become the dominant degradation sites; the first field evidence is usually brown streaks and loss of weld-line strength.
From a regulatory perspective, the compound can be supplied in RoHS-compliant formulations under EU Directive 2011/65/EU, with no intentionally added lead, mercury, cadmium, hexavalent chromium, PBB, or PBDE beyond Annex II thresholds. REACH registration is required for the polymer and monomer in the EU supply chain; finished articles must be screened against the Candidate List of substances of very high concern. For food-contact applications, the raw-material grade alone does not establish compliance; the finished part must be evaluated under EU Regulation No 10/2011 for overall migration and specific migration limits. Migration kinetics in the polymer matrix are influenced by low-molecular-weight residues and by the glass-fibre sizing. The grade is not recommended for prolonged contact with esters, ketones, or strongly alkaline aqueous solutions at elevated temperature. Addition of external regrind with unknown additive packages is not recommended above 25% by weight in critical applications.