Basf Ultradur Pbt Gf B 4500

BASF Ultradur® PBT+GF B 4500

    • Product Name: BASF Ultradur® PBT+GF B 4500
    • Factroy Site: Yinchuan, Ningxia, China
    • Price Inquiry: sales8@ascent-chem.com
    • Manufacturer: Ascent Petrochem Holdings Co., Limited
    • CONTACT NOW
    VTB
    Specifications
    HS Code 221248
    Density G Cm3 1.53
    Glass Fiber Content Percent 30
    Tensile Modulus Mpa 10000
    Tensile Strength Mpa 135
    Elongation At Break Percent 2.5
    Charpy Notched Impact Strength Kj M2 8
    Hdt A C 205
    Vicat B C 220
    Water Absorption Percent 0.4
    Mold Shrinkage Percent 0.3-0.8
    Melt Temperature C 250-270
    Mold Temperature C 60-100

    As an accredited BASF Ultradur® PBT+GF B 4500 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing BASF Ultradur® PBT+GF B 4500 is packaged in 25 kg moisture-barrier bags, supplied on pallets for safe industrial storage and handling.
    Container Loading (20′ FCL) BASF Ultradur® PBT+GF B 4500 loaded in a 20-foot FCL container, palletized and secured for safe ocean transport.
    Shipping BASF Ultradur® PBT+GF B 4500 is supplied as glass-fiber-reinforced PBT pellets in moisture-proof bags or octabins. It is not classified as dangerous goods for transport. Ship under dry conditions, protect from moisture and excessive heat, and follow SDS/labeling requirements.
    Storage Store BASF Ultradur® PBT+GF B 4500 in a cool, dry, well-ventilated area away from direct sunlight, heat sources, and open flames. Keep containers tightly closed to prevent moisture absorption and contamination. Avoid dust generation and static buildup. Maintain good housekeeping, proper labeling, and follow local regulations and the manufacturer’s safety data sheet.
    Shelf Life BASF Ultradur® PBT+GF B 4500 has a shelf life of 12 months from delivery when stored dry, sealed, below 30°C, and away from moisture and heat.
    Free Quote

    Competitive BASF Ultradur® PBT+GF B 4500 prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.

    We will respond to you as soon as possible.

    Tel: +8618005193850

    Email: sales8@ascent-chem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    BASF Ultradur® PBT+GF B 4500 is a short-glass-fiber-reinforced polybutylene terephthalate injection-molding compound classified within the medium-viscosity Ultradur B series. The matrix is produced by polycondensation of 1,4-butanediol with terephthalic acid or dimethyl terephthalate, and the glass-fiber package is introduced by melt compounding on a co-rotating twin-screw extruder. When specified as PBT+GF, the grade is typically supplied with a nominal glass-fiber loading of 10 wt%; lot-specific reinforcement content is determined by ISO 3451-1 ignition-loss analysis, and the certificate of analysis is the controlling document for substitution decisions. The compound is used for thin-wall connector bodies, coil shells, relay bases, sensor housings, and structural carriers in which dimensional stability at elevated temperature must be combined with short cycle times and low moisture uptake. The values below are expressed using ISO documentation because the grade is supplied in Europe and Asia with DIN EN ISO 527, ISO 178, ISO 179, and ISO 75 data packages.

    What Limits the Processing Window When B 4500 Is Run on Hot-Runner Tools?

    Pre-drying is mandatory at 120 °C for 4 h in a desiccant dryer with a dew point of -40 °C or lower; residual moisture must remain below 0.02 wt% because the ester linkages in the PBT backbone undergo hydrolytic chain scission in the barrel. In hot-runner tools with restricted flow channels, moisture-related surface splay and a drop in notched Charpy impact strength from 4.0 kJ/m² to approximately 2.8 kJ/m² can occur when the dryer dew point drifts above -30 °C. Melt-temperature settings should be maintained between 250 °C and 275 °C at the nozzle, with barrel zones distributed from 240 °C rear to 265 °C front. Mold-surface temperature is normally controlled between 60 °C and 100 °C; below 60 °C crystallization is too slow for full shrinkage compensation, while above 100 °C cycle-time benefits are lost and flash risk increases on low-clamp machines. The melt volume-flow rate of 13 cm³/10 min at 250 °C and 2.16 kg permits filling of wall sections down to 0.8 mm, but the temperature window narrows when hot-runner manifolds are used. External heating is preferred over internal torpedo heaters because dead spots above 280 °C initiate thermal degradation of the glass-fiber sizing and yellowing of the compound. Residence time should not exceed 8 min at 270 °C; cumulative residence beyond 12 min produces measurable reductions in tensile stress at break under ISO 527-1/-2. Injection velocity should be held in the range 100–300 mm/s, and hold pressure between 50 MPa and 80 MPa is required to prevent sink marks at fiber-rich weld lines. Screw back pressure of 3–7 bar assists melt homogeneity without excessive fiber-length reduction.

    PropertyStandard methodRepresentative value
    Density at 23 °CISO 1183-11.37 g/cm³
    Melt volume-flow rate, 250 °C/2.16 kgISO 1133-113 cm³/10 min
    Tensile modulus, 1 mm/minISO 527-1/-25000 MPa
    Tensile stress at break, 5 mm/minISO 527-1/-290 MPa
    Tensile strain at breakISO 527-1/-23.5%
    Flexural modulus, 2 mm/minISO 1784500 MPa
    Flexural strengthISO 178140 MPa
    Charpy notched impact strength, 23 °CISO 179/1eA4.0 kJ/m²
    Charpy unnotched impact strength, 23 °CISO 179/1eU45 kJ/m²
    Heat deflection temperature A, 1.8 MPaISO 75-1/-2200 °C
    Heat deflection temperature B, 0.45 MPaISO 75-1/-2220 °C
    Melting temperature, DSCISO 11357-1/-3223 °C
    Vicat softening temperature, 50 N, 50 °C/hISO 306205 °C
    Molding shrinkage, parallel/normalISO 294-40.5/1.0%
    Water absorption, saturation at 23 °CISO 620.4%
    Flammability at 1.6 mm thicknessUL 94HB

    Substitution of PBT+GF B 4500 for an unfilled PBT such as Ultradur B 4520 changes the mechanical response from ductile to semi-ductile. Tensile modulus increases from approximately 2600 MPa to 5000 MPa when measured at 1 mm/min under ISO 527-1/-2, while tensile strain at break falls from above 15% to 3.5%. Heat deflection temperature A rises from below 60 °C for unfilled PBT to 200 °C at 1.8 MPa for the glass-reinforced grade, which explains why B 4500 is selected for connectors that must survive wave soldering and infrared reflow profiles peaking at 250 °C. Compared with higher-glass Ultradur B 4300 G4 and G6 grades, B 4500 PBT+GF provides lower warpage and better surface gloss at the expense of tensile modulus and notched impact. The notched Charpy impact strength of 4.0 kJ/m² at 23 °C is lower than that of a 30 wt% glass grade, which can reach 8–10 kJ/m²; therefore B 4500 is not the first choice for snap-fit designs requiring high post-mold toughness. Dimensional-change data from ISO 294-4 show parallel shrinkage of 0.5% and normal shrinkage of 1.0%, producing an anisotropy ratio of approximately 2:1 that must be compensated by gate placement in flat housings. Water absorption of 0.4% at saturation under ISO 62 supports stable electrical properties in humid environments, but the glass-fiber sizing can still contribute to blistering if pellets are exposed to ambient air above 60% relative humidity without drying.

    If Fiber-Length Retention Is Prioritized Over Throughput, Screw Design Becomes Controlling

    Compounding of B 4500 PBT+GF on a co-rotating twin-screw extruder with L/D 40:1 and a side feeder located at 9D from the feed throat demonstrates the conflict between dispersion and fiber preservation. When glass roving is fed downstream at 400 rpm screw speed, the median fiber length after pelletizing is typically 0.25–0.35 mm; increasing screw speed to 700 rpm raises throughput but reduces median fiber length to 0.15–0.20 mm and lowers notched Charpy impact strength by approximately 15%. Kneading blocks with 45° staggering and two neutral elements are used to open the glass bundles, but excessive reverse elements increase melt temperature above 280 °C and accelerate degradation of the PBT matrix. Vacuum venting at -0.08 MPa is applied after the side feeder to remove volatiles and maintain an oligomer level low enough to avoid plate-out on mold surfaces. Melt filtration through a 60/100 mesh screen pack is recommended before pelletizing; pressure build-up above 120 bar at the screen changer indicates fiber agglomeration and inadequate wetting. For injection molders, pellet geometry, packing density, and glass-fiber length distribution should be monitored because batch-to-batch variance in median fiber length can shift the notched Charpy value by 0.5–1.0 kJ/m² even when the formulation is unchanged.

    Electrical Tracking, Thermal Aging, and Regulatory Compliance Boundaries

    Electrical components molded from B 4500 PBT+GF require comparative tracking index confirmation by IEC 60112. Glass reinforcement lowers tracking resistance relative to unfilled PBT; a high-CTI connector application often requires a special stabilizer package. Thermal endurance for electrical insulation systems is evaluated under IEC 60216-1 and the UL 746B relative thermal index; the assigned RTI is specific to color and wall thickness and must be taken from the UL Yellow Card for the supplied grade. Dimensional stability under combined thermal and electrical load is characterized by ISO 75-1/-2 HDT A at 1.8 MPa and by IEC 60695-2-12 glow-wire testing if the final article is used in unattended household appliances.

    The compliance status of the supplied pellet is defined by the regulatory documents listed below. Lot-specific declarations should be requested for every production batch because colorants, glass sizing, and processing aids are part of the final compound.

    Regulatory areaStandard or clauseVerification basis
    RoHS restricted substancesEU Directive 2011/65/EU Annex II, (EU) 2015/863Lead, mercury, cadmium, hexavalent chromium, PBB, PBDE, DEHP, BBP, DBP, and DIBP below 0.1 wt%; cadmium below 0.01 wt% in homogeneous material
    REACH SVHC declarationRegulation (EC) No 1907/2006, Article 57Statement of compliance against the current candidate list
    Food-contact resin statusFDA 21 CFR 177.1660Applicable to PBT resin; glass fiber, colorants, and processing aids require separate evaluation
    Plastic food-contact materialsCommission Regulation (EU) No 10/2011 Annex IOverall migration limit of 10 mg/dm² must be validated on the finished article
    Flammability classificationUL 94HB at 1.6 mm unless a flame-retardant variant is specified
    Electrical insulation thermal enduranceIEC 60216-1 and UL 746BRTI from UL Yellow Card for the specific color and thickness

    For repeated food-contact use, 21 CFR 177.1660 covers polybutylene terephthalate resin, but the glass-fiber reinforcement and any external lubricants must be evaluated separately under the intended conditions of use. Electrical grades are not automatically food-contact grades, and migration testing according to Commission Regulation (EU) No 10/2011 Annex V remains mandatory on the finished part if the application involves repeated food contact or potable water exposure.