| HS Code | 671731 |
| Product | BASF Ultradur® PBT+GF B 4300 G6 |
| Polymerbase | Polybutylene terephthalate (PBT) |
| Reinforcement | Glass fiber |
| Glassfibercontent | 30% |
| Density | 1.53 g/cm³ |
| Tensilemodulus | 9500 MPa |
| Tensilestrength | 140 MPa |
| Elongationatbreak | 2.5% |
| Charpynotchedimpactstrength23c | 8 kJ/m² |
| Hdt A | 205 °C |
| Hdt B | 220 °C |
| Meltingpoint | 223 °C |
| Moldshrinkage | 0.3–0.8% |
| Melttemperature | 250–275 °C |
| Moldtemperature | 60–100 °C |
| Waterabsorptionsaturation | 0.4% |
As an accredited BASF Ultradur® PBT+GF B 4300 G6 factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Packaged in 25 kg moisture-barrier paper bags on pallets, BASF Ultradur® PBT+GF B 4300 G6 offers safe handling and storage. |
| Container Loading (20′ FCL) | 20′ FCL dry container loaded with palletized 25 kg bags of BASF Ultradur® PBT+GF B 4300 G6, securely strapped and evenly distributed. |
| Shipping | BASF Ultradur® PBT+GF B 4300 G6 is shipped as non-hazardous thermoplastic pellets in sealed moisture-barrier bags or octabins. No UN number or dangerous-goods classification applies. Keep dry, avoid prolonged heat/UV exposure, and handle under normal industrial hygiene practices. |
| Storage | Store BASF Ultradur® PBT+GF B 4300 G6 in a cool, dry, well-ventilated area, preferably in original sealed moisture-barrier bags or containers. Protect from direct sunlight, heat, and humidity. Keep containers closed and avoid contact with incompatible chemicals. If moisture uptake is suspected, dry the pellets according to the supplier’s processing recommendations before use. |
| Shelf Life | Shelf life is about 24 months when stored dry in sealed original packaging at room temperature, away from moisture and direct sunlight. |
Competitive BASF Ultradur® PBT+GF B 4300 G6 prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
BASF Ultradur® B 4300 G6 is a 30% glass-fibre reinforced polybutylene terephthalate injection moulding compound classified within the B 4300 series. The product is supplied in cylindrical granule form and is processed on standard reciprocating-screw injection moulding machines. The glass reinforcement is short fibre, not long fibre; the moulded part therefore retains flowability through thin-wall gates but develops anisotropic mechanical properties in relation to the melt-fill direction. Density is typically 1.53 g/cm³ under ISO 1183-1, melt volume rate is approximately 9 cm³/10 min at 250 °C under a 2.16 kg load according to ISO 1133-1, and the melting peak by differential scanning calorimetry is approximately 223 °C according to ISO 11357-3. The product is not a flame-retarded compound and is normally rated HB under UL 94 at 1.5 mm thickness. It is used in connectors, sensor bodies, small actuator housings, and gear carriers where dimensional stability, fuel and oil resistance, and high stiffness in snap-fit assembly are required.
| Property | Standard method | Typical value |
|---|---|---|
| Density | ISO 1183-1 | 1.53 g/cm³ |
| Tensile modulus | ISO 527-2 | 10,000 MPa |
| Tensile stress at break | ISO 527-2 | 140 MPa |
| Flexural modulus | ISO 178 | 9,500 MPa |
| Flexural strength | ISO 178 | 220 MPa |
| Charpy notched impact | ISO 179/1eA | 10 kJ/m² at 23 °C |
| Charpy unnotched impact | ISO 179/1eU | 55 kJ/m² at 23 °C |
| Heat deflection temperature A | ISO 75-2/A | 205 °C |
| Heat deflection temperature B | ISO 75-2/B | 220 °C |
| Melting temperature | ISO 11357-3 | 223 °C |
| Mould shrinkage, parallel | ISO 294-4 | 0.3 % |
| Mould shrinkage, transverse | ISO 294-4 | 1.0 % |
| Water absorption, 24 h | ISO 62 | 0.2 % |
| Volume resistivity | IEC 62631-3-1 | >1E13 Ω·m |
| Surface resistivity | IEC 62631-3-2 | >1E15 Ω |
These values are typical and should not be read as specification minima; pigment packages, regrind content, and moulding conditions can shift the tensile modulus by ±5 % and the notched impact by at least ±10 %. First-article evaluation using moulded plaques conditioned at 23 °C and 50 % relative humidity for 48 h according to ISO 291 is preferable to raw granulate specification review.
Within the B 4300 series, the G-code defines the nominal glass fibre content: G2 = 10 %, G4 = 20 %, G6 = 30 %, G8 = 40 %, and G10 = 50 %. The difference between B 4300 G6 and lower-glass counterparts is not limited to stiffness. Raising the fibre content to 30 % increases flexural modulus and heat deflection temperature while lowering the coefficient of linear thermal expansion in the flow direction. It also raises the melt viscosity and makes the fracture behaviour more notch sensitive at weld lines and at sharp corners. The short-fibre orientation distribution produced by the melt front in a 2 mm wall section creates a tensile modulus gap between the flow direction and the cross-flow direction; this gap is larger in G6 than in G4. Relative to G4, B 4300 G6 produces higher tool and barrel abrasion; the increased glass concentration demands screw, barrel, and non-return valve surfaces with abrasion-resistant hardfacings or carbide-modified alloys. Some processors specify a bimetallic barrel with a hardness above 60 HRC and a screw flight hardfacing of cobalt- or nickel-base alloy to extend service intervals when running long production campaigns.
Relative to G10, the intermediate glass content of B 4300 G6 preserves lower melt viscosity and lower density, which reduces shot weight and clamp force demand for the same cavity geometry. A 30 % glass-filled material also generates less abrasion on gate inserts and ejector sleeves than a 50 % glass-filled grade. However, G10 offers higher flexural modulus and lower mould shrinkage than G6 when part flatness requirements are extreme. The selection between G6 and G10 for a housing with a long, slender bayonet feature is therefore a trade-off between filling pressure and post-mould geometry. In a spiral flow comparison under identical melt and mould temperatures, the 30 % glass grade displays a shorter flow path than G4 and a longer flow path than G10; the exact ratio depends on the hot-runner pressure drop and the crystallisation rate at the mould surface. This intermediate position makes B 4300 G6 suitable for thin-wall connector bodies above 0.8 mm wall thickness where G10 would create short shots or gate blush and G4 would allow excessive post-mould warpage after moisture absorption.
For failure analysis and material acceptance, the glass content can be checked by ash content using thermogravimetric analysis according to ISO 3451-1; the residual ash typically falls in the 28–32 % range. Fibre length distribution after injection moulding is commonly in the 150–350 µm range for short-glass PBT processed within the recommended screw-speed window; this distribution shifts below 120 µm if aggressive screw rotation and back pressure are used. In a thin-wall connector housing, the fibre orientation can be assessed by polishing a cross-section and measuring the orientation tensor rather than by simple visual inspection. These measurements are not needed for routine part release, but they are used when notched impact or weld-line strength fails a functional test after process parameter changes.
Drying is the principal pre-processing constraint for BASF Ultradur® B 4300 G6 because PBT is hydrolytically sensitive at melt temperature. The granulate must be dried to a residual moisture content below 0.04 %. A closed-loop desiccant dryer with a dew point between −40 °C and −50 °C should supply air at 80 °C for 4 h when starting from sealed bags. If the granulate has been exposed to ambient air above 60 % relative humidity for more than 30 min, the drying time should be extended to 6 h and the hopper should be purged with dry air. The melt temperature window is 250–270 °C; rear barrel zones are held at 240–250 °C, middle zones at 250–260 °C, and the nozzle at 260–270 °C. The mould surface temperature should be set to 60–100 °C. At a mould surface temperature below 60 °C, the fast-crystallising PBT matrix freezes before full packing, producing sink marks and high injection pressure. At a mould surface temperature above 100 °C, the cycle time increases and cross-flow shrinkage may increase.
Thermal degradation becomes measurable above 280 °C. The ester backbone releases volatile by-products, and the melt viscosity drops in proportion to molecular weight loss. A melt residence time above 8 min should be avoided; this is particularly important with large shot weights and small screw sizes because the plastication capacity may be severely oversized. Screw rotation speed should be limited to 30–80 m/min peripheral speed, and back pressure should be set between 3 MPa and 7 MPa to improve melt homogeneity without excessive fibre attrition. A three-section, low-compression screw with a smear tip and a positive shut-off nozzle is preferred. Hot-runner manifolds should be heated below 270 °C; dead spots and low-flow channels should be eliminated because stagnating melt generates black specks and causes viscosity drift. Regrind addition above 20 % is not recommended for precision housings because regrind shortens the fibre length distribution and reduces notched impact strength. If regrind is used, it should be dried under the same conditions as virgin material and introduced in a separate gravimetric feeder rather than tumbled into the virgin granulate.
Heat deflection temperature is approximately 205 °C under 1.8 MPa and 220 °C under 0.45 MPa according to ISO 75-2. The melting peak is 223 °C. These values are short-term test values and do not represent a continuous use limit. In air, short-glass PBT of this class is generally limited to 130–140 °C continuous service, with short-term excursions to 160 °C only when mechanical stress is low and the part is not under high clamp load. In hot aqueous environments, hydrolysis is the controlling degradation route rather than oxidation. Continuous immersion in water or water-glycol coolant above 60–80 °C is an application boundary for stress-critical parts. Under alkaline conditions above pH 9, ester bond cleavage accelerates, and the molecular weight loss appears first as reduced weld-line strength and reduced melt viscosity in regrind evaluation. The product is not recommended for continuous exposure to strong acids or strong alkaline cleaning baths above 10 % concentration at elevated temperature. Published data for this specific configuration under continuous automotive coolant immersion is limited; a supplier-run chemical ageing study is required before qualifying a sensor body for long-term underhood glycol contact.
Typical electrical values include volume resistivity greater than 1E13 Ω·m and surface resistivity greater than 1E15 Ω. Comparative tracking index is generally reported in the 250–300 V range under IEC 60112 for 30 % glass-filled PBT without flame-retardant additives. The glass fibres reduce dielectric strength relative to unfilled PBT; fibre ends and moulded-in voids can become charge concentration sites under high DC voltage. For connectors operating above 48 V, creepage and clearance distances should follow IEC 60664-1, with pollution degree 2 or 3 verified on moulded samples. Surface treatments with polar cleaning agents or plasma may temporarily reduce surface resistivity; therefore, electrical tests should be performed on samples that have not been cleaned with isopropanol immediately before measurement. The supplier declaration covers RoHS Directive 2011/65/EU and the REACH candidate list for the relevant production site.
In automotive electrical distribution and actuator applications, BASF Ultradur® B 4300 G6 is used for connector bodies, sensor flanges, relay covers, fuse boxes, window or seat motor gear carriers, and electronic control unit housings. The material withstands aliphatic hydrocarbons, diesel fuel, glycol, automatic transmission fluid, and mineral oil at atmospheric pressure. Aromatic solvents, ketones, and concentrated organic acids are not recommended. The 30 % glass filler produces anisotropic mould shrinkage: approximately 0.3 % in the flow direction and 1.0 % cross-flow when measured on a 60 mm × 60 mm × 2 mm plaque according to ISO 294-4. The anisotropy forces gate placement along the least tolerance-sensitive axis; it also means that radial ribs, bosses, and snap-fit hooks should be aligned to the flow direction where possible. In multi-cavity tools with more than 16 cavities, cavity-to-cavity variation in glass content can range from 27 % to 33 % when cavity flow lengths are dissimilar; the resulting tensile modulus difference between first and last filled cavities can be 2–5 %. The material can be ultrasonically welded, laser marked, and hot-plate welded. Adhesive bonding generally requires surface activation by plasma or flame treatment if a lap-shear strength above 5 MPa is required on as-moulded surfaces, because the glass-reinforced PBT surface has low surface free energy.
Because the material is used in snapped assemblies and gear carriers, short-term strength alone does not govern service performance. The flexural modulus of 9,500 MPa under ISO 178 provides high bending stiffness, but the creep modulus under sustained load decreases with time and temperature. Published data for this specific grade under combined vibration and thermal ageing is limited; moulded prototype parts should be fatigue tested according to the automotive customer’s vibration profile. Snap-fit designs should limit strain in the corner fibres to the low single-digit percentage range to prevent glass-fibre breakage during assembly.
When a housing requires multiple gates around a central opening, the weld line is the controlling design feature in glass-fibre reinforced PBT. At the weld front, glass fibres orient predominantly along the flow direction and transverse to the weld plane; the weld zone is matrix-dominated and cannot transfer load through the glass reinforcement. In 30 % glass-filled PBT, weld-line tensile strength is typically reduced by 30–50 % relative to an unwelded specimen when tested according to ISO 527-2. The reduction is not linear with glass content: below 20 % glass the weld retains more bulk strength, while above 40 % glass the weld zone may become a brittle plane with additional porosity and microcracking. For B 4300 G6, mould-filling simulation of a 2 mm-thick connector clip with a central core hole has been used to reposition two side gates to a single end gate. This changes the weld-line location away from the snap-fit root and reduces the probability of field cracking during repeated engagement. The flow front temperature at the end of fill should not fall below 240 °C; for long flow paths, a mould surface temperature of at least 80 °C is necessary to prevent premature solidification of the flow front. Packing pressure can be raised to 60–80 MPa hydraulic line pressure for 0.5–1.5 s after switchover to compress the weld plane and reduce V-notch formation. If weld-line strength remains insufficient, the preferred changes are gate relocation, flow leader geometry, or local thickness adjustment. Increasing mould temperature to 120 °C is not a generic cure; it shifts crystalline morphology and may increase cross-flow shrinkage by approximately 0.2 % without proportional weld strength gain. The use of high-speed injection to raise shear heating at the flow front can shorten the process window; excessive shear can cause surface blistering and fibre-free skins on the melt front.