| HS Code | 880109 |
| Density | 0.918 g/cm³ |
| Melt Index 190 C 2 16 Kg | 1.0 g/10 min |
| Tensile Strength At Break Md | 5,000 psi |
| Tensile Strength At Break Td | 4,500 psi |
| Tensile Strength At Yield Md | 1,200 psi |
| Elongation At Break Md | 500% |
| Elongation At Break Td | 600% |
| Dart Drop Impact | 200 g |
| Elmendorf Tear Strength Md | 200 g/mil |
| Elmendorf Tear Strength Td | 400 g/mil |
| Haze | 10% |
| Gloss 45 | 70% |
| Melting Point | 120°C |
| Vicat Softening Point | 95°C |
| Coefficient Of Friction | 0.20 |
As an accredited Bamberger Polymers Bapolene® 610P LLDPE, Metallocene Film Grade factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Supplied in 25 kg (55.1 lb) polyethylene-lined paper bags, palletized, or 1,000 kg bulk bags for industrial shipment. |
| Container Loading (20′ FCL) | 20′ FCL: approximately 18 MT (720 x 25 kg bags) of Bapolene 610P LLDPE metallocene film grade, depending on carrier. |
| Shipping | Bamberger Polymers Bapolene® 610P LLDPE, Metallocene Film Grade, is shipped as a non-hazardous solid, typically in 25 kg polyethylene bags or bulk containers. Pallets are stretch-wrapped and labeled. Transport in clean, dry vehicles. Store away from moisture, heat, and direct sunlight. No special DOT placarding required. |
| Storage | Store Bamberger Polymers Bapolene® 610P LLDPE, Metallocene Film Grade, in a cool, dry, well-ventilated warehouse at ambient temperature. Keep original packaging closed and off the floor, away from direct sunlight, heat, ignition sources, moisture, and strong oxidizers. Avoid contamination and prolonged UV exposure. Use first-in, first-out stock rotation. Follow manufacturer/SDS storage guidance. Do not store outdoors or near incompatible materials. |
| Shelf Life | Shelf life is typically 12 months from manufacture when stored in original unopened packaging in a cool, dry, well-ventilated place. |
In cast film extrusion for 12–35 µm machine-grade pallet stretch film, Bapolene® 610P is run on 90–110 mm single-screw extruders with a 30:1 L/D ratio and barrier flight screw geometry. The resin’s nominal melt index of 1.0 g/10 min (ISO 1133-1:2022) and density of 0.918 g/cm³ (ISO 1183-1:2019) set the initial melt temperature profile. Melt temperature is held between 195°C and 230°C, depending on line speed, while the flat die gap is set at 0.5–0.8 mm. The melt curtain is pinned onto a chrome-plated chill roll maintained at 18–28°C; higher chill roll temperatures are introduced only when the film receives a post-calendered embossing or cling additive layer. Draw resonance becomes observable when line speed exceeds 280–350 m/min if the die gap is narrowed below 0.4 mm or if melt strength is insufficient. A fluoropolymer processing aid masterbatch at 0.02–0.08 phr suppresses die-lip build-up and reduces melt fracture in the 200–400 s⁻¹ shear range. The formulation uses Bapolene® 610P as the base resin at 70–100 wt%; the remainder is either a lower-density metallocene plastomer at 10–30 wt% to increase film stretch and clamp retention, or a fractional-melt LDPE at 10–20 wt% to improve draw stability on cast lines without automated thickness control. Compliance references include FDA 21 CFR 177.1520(b)(3) when the film is intended for indirect food contact in transit packaging, EU Regulation (EU) No 10/2011 Annex I with the overall migration limit of 10 mg/dm² for food-contact pallet wrapping, and REACH SVHC screening. Mechanical verification on the finished film is performed according to ASTM D882-18 for tensile elongation, ASTM D5748-19 for puncture resistance, and ASTM D5458-95(2012) for cling when a tackifier layer is present. Terminal product types include hand stretch film at 15–23 µm, machine stretch film at 20–35 µm, pre-stretched wrap at 8–15 µm, and agricultural bale wrap when UV masterbatch is separately added at 1–3 wt%.
On cast stretch film lines, the primary process conflict is the interaction between chill roll temperature and cling additive bloom. When tackifier is compounded into the melt, chill roll temperatures above 28°C accelerate surface migration and produce non-uniform cling, while temperatures below 18°C increase film stiffness and reduce pre-stretch activation. Winder tension taper is set from 10% to 40% of initial web tension to prevent blocking and telescoping. Edge trim from the line is typically reintroduced at 5–15 wt% only when the trim is dry and free of silicone oil contamination; higher reuse rates shift dart impact and puncture resistance outside the target specification.
When Bapolene® 610P replaces a conventional Ziegler-Natta LLDPE in food-consumer blown film, the narrower molecular weight distribution changes the shear and melt strength balance. On a 55–75 mm grooved-feed extruder with a 30:1 L/D ratio and a 200–350 mm annular die, the die gap is typically widened to 1.5–2.5 mm to prevent melt fracture. Melt temperature is controlled between 190°C and 230°C. The bubble is run at a blow-up ratio of 2.0:1–3.0:1, with frost line height maintained at 4–8 die diameters; dual-lip air rings or internal bubble cooling are required when output exceeds 180 kg/h. Bubble instability is most frequently recorded when frost line height drops below 3 die diameters or when the melt temperature exceeds 240°C, producing visible gauge bands and poor roll conformation. The base resin is used at 100 wt% or blended with a high-pressure LDPE at 10–20 wt% to increase bubble stability. Antiblock masterbatch is added at 0.5–1.5 wt%, slip erucamide at 0.05–0.20 wt%, and fluoropolymer processing aid at 0.02–0.06 phr. Food-contact compliance is evaluated under FDA 21 CFR 177.1520(b)(3) and EU Regulation (EU) No 10/2011 Annex I, with overall migration limited to 10 mg/dm². Finished film is tested for dart impact according to ISO 7765-1:1988 or ASTM D1709-16ae1, tear according to ISO 6383-2:1983 or ASTM D1922-15(2020), haze according to ASTM D1003-21, and gloss according to ASTM D2457-21. Terminal products include bread bags, fresh produce films, frozen vegetable pouches, and general food storage bags in thicknesses from 20 µm to 80 µm.
On the same blown film line, the resin’s processing window is bounded on the upper side by gel formation above 250°C and on the lower side by screw torque rise below 175°C. Extruder screens are specified at 60/80/100 mesh to capture char particles and slightly increase head pressure; a pressure drop greater than 80 bar across the screen pack indicates the need for a change. Bubble cooling air temperature should remain below 12°C when film haze below 8% is required, because slow crystallization in thick sections increases surface haze and lowers gloss below 60 GU at 45° geometry.
As a sealant web in dry-bond lamination, Bapolene® 610P is extruded as a 30–60 µm film and bonded to BOPP, PET, or aluminium foil using solventless polyurethane adhesive applied at 1.5–2.5 g/m². The laminating nip is held at 60–80°C, and the wound reel is cured for 24–48 h at 40–50°C before seal strength testing. The sealant formulation uses Bapolene® 610P at 100 wt% or in a blend with a metallocene plastomer at 10–30 wt% to reduce seal initiation temperature. Seal jaw temperatures on horizontal form-fill-seal equipment are set between 115°C and 160°C; above 160°C, seal thinning and tear propagation at the seal edge become measurable. Compliance references include EU Regulation (EU) No 10/2011 Annex I for plastic materials in food contact and FDA 21 CFR 177.1520(b)(3) for the olefin polymer layer. Seal strength is verified according to ASTM F88/F88M-21, hot tack according to ASTM F1921-12(2018), and lamination bond strength according to ASTM D903-98 or ISO 11339:2022. Terminal finished products include stand-up pouches, zipper pouches, quad-seal bags, and dry food flow-wrap packs. The configuration is not recommended for retort conditions above 100°C core product temperature, because seal creep becomes the limiting failure mode.
Adhesive compatibility is checked by measuring lamination bond strength after 24 h cure; values below 2.0 N/15 mm are traced either to corona treatment losses on the film surface below 38 mN/m or to plasticizer migration from the sealant. Corona discharge is applied inline at 0.8–1.2 kW per metre width. Because the 610P sealant layer is non-polar, surface oxidation must be verified by ASTM D2578-17 wetting tension measurements immediately before lamination.
In frozen food packaging, Bapolene® 610P is blended with a metallocene plastomer at 10–30 wt% to shift the seal initiation temperature downward and improve impact resistance at -20°C. The base resin content is 70–90 wt%, with slip and antiblock masterbatch additions held at 0.5–1.5 wt% because higher antiblock loadings reduce low-temperature seal strength. Film is produced on 3-layer blown film lines with skin layers containing the 610P-plastomer blend and a core layer of conventional LLDPE or recycled trim at 20–40 wt%. Die gap is set at 1.8–2.5 mm, blow-up ratio at 2.0:1–2.8:1, and melt temperature at 190–230°C. Frost line height is kept above 5 die diameters to preserve dart impact resistance above 800 g at 50 µm thickness in ASTM D1709-16ae1 testing; published data for this specific configuration is limited and should be verified on the target line. Low-temperature film strength is measured by ASTM D882-18 at -18°C, and seal strength after frozen conditioning is checked with ASTM F88/F88M-21. Compliance for direct food contact remains under FDA 21 CFR 177.1520(b)(3) and EU Regulation (EU) No 10/2011 Annex I, with the overall migration limit of 10 mg/dm². Terminal products include frozen vegetable pouches, ice cream bags, frozen meat films, and frozen pastry overwrap.
On vertical form-fill-seal machines, frost contamination on the seal area is a documented cause of seal strength loss; seal jaws are maintained at 120–155°C, with dwell time at 0.3–0.8 s and pressure above 3 bar. When product surface temperature is below -25°C, seal strength drops unless a wider seal bead of at least 5 mm is used. Films containing 20–30 wt% plastomer exhibit lower hot tack but improved cold seal ductility.
Bapolene® 610P is used as the outer and inner skin layers of 25–75 µm silage bale wrap produced on 3-layer blown film lines. The formulation includes 1–3 wt% UV masterbatch, 2–4 wt% color masterbatch, and 0.5–1.5 wt% polyisobutylene tackifier for cling. Dispersive mixing is required because UV and pigment masterbatch agglomerates above 80 µm create film defects and reduce elongation retention. A Maddock mixing section or screw with a length of 24:1 or longer is specified. Die gap is 1.8–2.5 mm, blow-up ratio is 2.0:1–2.5:1, and melt temperature is held between 190°C and 225°C. Compliance references include EN 13206:2017 where applicable for agricultural film, REACH SVHC screening, and EU Regulation (EU) No 10/2011 Annex I only where silage contact may involve subsequent food chain exposure. Tensile properties are evaluated to ISO 527-3:2018 or ASTM D882-18, tear resistance to ASTM D1922-15(2020), and UV stabiliser dispersion by film appearance after 500 h of accelerated weathering. Terminal products include silage bale wrap, round bale cover, bunker silo cover, and greenhouse side film.
Because the film is not an oxygen barrier, silage fermentation is maintained by physical sealing and UV opacity rather than gas barrier performance. Thickness variation below ±5% is controlled by on-line gauge scanners; variation above this range creates uneven cling and premature aging at splice points. UV masterbatch dispersion is assessed by film appearance after 500 h of accelerated weathering according to ISO 4892-2:2021, with retained elongation above 50% as an acceptance reference.
For heavy-duty sack applications with thicknesses from 100 µm to 200 µm, Bapolene® 610P is blended with high-pressure LDPE at 20–40 wt% to raise melt strength and reduce bubble sag on 150–350 mm annular dies. Carbon black masterbatch is added at 2–4 wt% when solar opacity and pile storage stability are required. Extruder barrel temperatures are set 5–10°C higher than in thin-gauge food film to control melt viscosity, with the melt temperature limited to 230°C maximum to avoid gel formation. Die gap is maintained at 2.0–2.8 mm, blow-up ratio at 2.0:1–2.5:1, and frost line height at 5–8 die diameters. Compliance for industrial packaging falls under REACH SVHC screening and RoHS Directive 2011/65/EU for heavy metals; food-contact sacks are additionally assessed under FDA 21 CFR 177.1520(b)(3) and EU Regulation (EU) No 10/2011 Annex I. Puncture resistance is evaluated by ASTM D5748-19, dart impact by ISO 7765-1:1988 or ASTM D1709-16ae1, and tear by ISO 6383-2:1983. Terminal products include fertilizer bags, polymer resin sacks, construction aggregate bags, and sandbags. Published data for this specific thickness range with Bapolene® 610P is limited; converter trials should confirm minimum dart impact target of 400 g at 150 µm before commercial approval.
Extruder screw torque and melt pressure rise are monitored at 150–220 bar head pressure; pressure above 250 bar indicates carbon black masterbatch agglomeration or screen blockage. The use of a 60/100/120 mesh screen pack reduces char contamination in thick film, but raises melt temperature by 2–5°C. Blending LDPE above 40 wt% lowers puncture resistance, while below 20 wt% bubble instability and gauge variation exceed ±8%.
Competitive Bamberger Polymers Bapolene® 610P LLDPE, Metallocene Film Grade prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Bamberger Polymers supplies Bapolene® 610P as a metallocene-catalyzed linear low-density polyethylene film resin. The grade is identified by a nominal density of 0.918 g/cm³ when tested in accordance with ASTM D1505 and a melt index of 1.0 g/10 min when measured at 190°C under 2.16 kg load in ASTM D1238. This placement in the LLDPE density and melt-viscosity envelope is intended for blown film and cast film used in flexible packaging, industrial liners, and laminated web structures. The metallocene catalyst system differentiates the resin from conventional Ziegler-Natta LLDPE grades by producing a narrower molecular weight distribution and a more uniform short-chain branching distribution. Those architectural differences alter melt rheology, heat-seal response, draw-down behavior, and solid-state mechanical balance. In commercial use, the resin is frequently considered when a packaging structure requires improved toughness at low film gauge, reduced seal initiation temperature, or enhanced optical clarity relative to a conventional butene or hexene LLDPE of similar density and melt index. Because the resin belongs to the single-site catalyst family, process behavior is not identical to standard LLDPE; internal bubble cooling, die-gap selection, and haul-off tension must be adjusted when transitioning from a conventional Ziegler-Natta grade.
The differentiating mechanism is the distribution of molecular species and comonomer placement. In a conventional Ziegler-Natta LLDPE, the catalyst produces a comparatively broad molecular weight distribution with comonomer incorporation concentrated in the low-molar-mass fraction. That heterogeneous architecture lowers the observed melting peak and creates a crystalline population with wide lamellar thickness distribution. In metallocene-catalyzed LLDPE such as Bapolene 610P, the active site uniformity produces more statistically random comonomer placement across the chain population. The structural consequence is a narrower melting range and lower seal initiation temperature as measured on gradient heat-seal testers following ASTM F1921 or ASTM F88. The rheological consequence is a more Newtonian low-shear response and a sharper transition into shear-thinning flow. On a capillary rheometer following ISO 11443, this viscosity profile commonly produces lower shear sensitivity at very low shear rates and higher sensitivity at typical die-shear conditions compared with broad-molecular-weight LLDPE. On blown-film equipment, this translates into higher extruder pressure sensitivity to die gap and output changes, but also improved gauge uniformity when downstream conditions are stable.
The solid-state response reflects the same chain architecture. The uniform branch distribution permits stress-induced orientation to develop more evenly across the film web, which is associated with improved dart drop impact when measured according to ASTM D1709A and improved Elmendorf tear characteristics in ASTM D1922. Optical haze and gloss values measured under ASTM D1003 and ASTM D2457 are generally superior to those obtained from Ziegler-Natta LLDPE of the same density and melt index. However, the narrow molecular weight distribution also reduces melt strength and elongational strain-hardening at high take-off speeds. This limitation must be managed through extrusion temperature, die gap, and internal bubble cooling rather than through blending with high-molecular-weight LLDPE alone.
Before line qualification, the resin’s physical property envelope is typically screened using compression-molded or film-derived specimens. The values listed in Table 1 are frequently published as release-sheet or product-data-sheet values, but lot-specific certificates of analysis should be consulted for incoming resin acceptance because film mechanical properties depend on gauge, blow-up ratio, and cooling rate. Published data for specific film configurations is limited unless the processor generates multimodal line data on the target extruder.
| Property | Test method | Unit | Typical value |
|---|---|---|---|
| Density | ASTM D1505 | g/cm³ | 0.918 |
| Melt index | ASTM D1238, 190°C/2.16 kg | g/10 min | 1.0 |
| Melting peak temperature | ASTM D3418 | °C | 120 |
| Vicat softening temperature | ASTM D1525 | °C | 100 |
The density and melt index values are the primary grade-identification parameters for warehouse segregation and extrusion process setup. The thermal values indicate the thermal range at which primary crystalline melting begins to disappear under controlled heating. They do not by themselves define the heat-seal initiation temperature; seal initiation is determined separately on a film sample at defined dwell, pressure, and temperature using ASTM F1921 or a packaging converter’s internal gradient-seal protocol.
Internal bubble cooling systems introduce measurable changes in frost-line height and bubble stability when running Bapolene 610P in monolayer or multilayer blown film. The resin’s narrow molecular weight distribution produces a lower melt strength than conventional LLDPE of equal melt index. In practice, this means the bubble is more susceptible to fluttering when the blow-up ratio exceeds the stable operating window of the line or when the die-gap residence time is too short. On production-scale three-layer blown-film equipment with barrier screws and L/D ratios between 24:1 and 30:1, a practical starting melt temperature range for this density and melt-index class is 190°C to 230°C at the die. Die gaps between 1.5 mm and 2.5 mm are common for metallocene LLDPE, and the bubble is typically run at blow-up ratios of 2.0:1 to 2.5:1 to balance impact strength and tear resistance.
Because the resin has a comparatively flat low-shear viscosity curve, screw torque and die pressure respond strongly to changes in barrel temperature and throughput. A sudden increase in screw speed may produce a non-linear rise in die pressure due to the onset of shear-thinning at higher die shear rates. Melt pressure values are therefore best interpreted with melt-pressure transducers placed immediately before the screen changer and at the die entry. The use of fine screen packs, typically 40/60/80 mesh combinations, may raise melt temperature and lower output if contamination or gel content is not controlled. In high-output lines, the melt temperature should be measured with a needle pyrometer at the die exit because the polymer melt may not fully equalize temperature across the die gap when extrusion is pushed beyond the normal specific output of the screw.
Bubble stability is further controlled by the internal bubble cooling air flow and the external air ring profile. With metallocene LLDPE, high-velocity internal air streams can create low-amplitude oscillation at the frost line if the internal bubble pressure is not stable. A common adjustment is to increase the die-gap residence time by reducing output or widening the die gap, rather than reducing melt temperature below the point where melt fracture appears. The onset of melt fracture in this resin class can be identified by surface roughness near the die exit and should not be confused with gauge variation. If melt fracture occurs, the first corrective action is to raise the die temperature or reduce shear rate before modifying the air stream.
Heat-transfer limitations in high-speed cast film extrusion are similarly influenced by the resin’s crystallization rate and surface quenching response. Bapolene 610P can be drawn at high line speeds when the chill roll temperature and contact pattern are optimized. For cast film, a chill roll temperature of 20°C to 30°C with adequate roll contact is typical, and the air-knife position determines whether the web develops edge pinning defects. The lower melt strength of metallocene LLDPE requires a shorter draw distance between the die exit and chill roll; excessive draw distance allows neck-in and thickness unevenness. The resin’s narrow melting range contributes to rapid solidification when the melt contacts the chill roll, but the same property increases the sensitivity of cast film to thermal shrinkage if the take-off speed is changed abruptly. Film flatness on cast lines should be evaluated with on-line beta gauges or after slitting under standardized tension, not only with manual micrometer spot checks.
If a processor replaces a C4 Ziegler-Natta LLDPE sealant layer with Bapolene 610P in a three-layer or five-layer film, the first measured difference is usually a reduction in seal initiation temperature. Heat-seal response curves generated on gradient sealers per ASTM F1921 typically shift to lower temperature by several degrees Celsius for metallocene LLDPE of equal density and melt index. The magnitude depends on seal-bar dwell time, pressure, substrate thickness, and whether the seal is made film-to-film or film-to-surlyn or film-to-EVA. Hot-tack strength may also improve when measured according to ASTM F1921 at equivalent seal temperatures, but the processing window is not automatically broader. The sealant layer grade substitution also changes the interfacial adhesion characteristics in coextrusion because the metallocene resin can possess lower melt elasticity at the die; the tie layer or core layer may need to be adjusted to maintain layer uniformity.
The mechanical advantage of the substitution is most evident in downgauging studies. Because the metallocene resin provides higher dart drop impact for equal film thickness, the converter can evaluate a 10% to 20% reduction in overall gauge while maintaining the packaging line performance of the previous LLDPE structure. In drop testing on filled packages, the limiting failure mode may shift from film puncture to seal integrity, which requires reevaluation of the package design rather than a direct comparison of resin data sheets. Published data for this specific configuration is limited when the exact coextrusion ratios, corona treatment levels, and lamination adhesives are not controlled.
On the packaging line, the lower seal initiation temperature permits faster cycle time on vertical form-fill-seal and horizontal form-fill-seal machines because the sealing jaw residence time can be reduced only if the seal bar temperature and pressure remain within the machine’s calibrated range. The actual packaging speed increase depends on the thermal conductivity of the film composite, the sealant layer thickness, and the jaw geometry. Processors should not extrapolate a laboratory gradient-seal result to a production machine without running a sealing-capability study on the target line. If the film contains slip and antiblock additives, those additives migrate over time and can alter seal strength; this is a known limitation, and the package-ageing response should be tested after at least 24 h of storage at controlled temperature.
Food-contact status for polyolefin film resins is not determined by the density or melt index classification alone. The resin may be supplied with documentation addressing compliance to 21 CFR 177.1520 for olefin polymers, including the condition-of-use limitations applicable to specific food types and temperatures. For the European Union, compliance to Regulation (EU) No 10/2011 on plastic materials and articles intended to come into contact with food requires overall migration testing under defined simulant and time/temperature conditions. The supplier should confirm the product’s specific regulatory certificate of compliance for each application because additive packages and lot-specific contamination limits can vary. Table 2 summarizes a compliance checklist matrix that should be verified against the supplier documentation before commercial use.
| Standard or regulation | Relevant scope | Verification condition |
|---|---|---|
| FDA 21 CFR 177.1520 | Olefin polymers for food contact | Supplier confirmation of condition-of-use compliance |
| EU No 10/2011 | Plastic materials in food contact | Overall migration and specific migration limits under defined simulants |
| REACH | Registration and authorization in EU | Registration number and safety data sheet confirmation |
| RoHS Directive 2011/65/EU | Restriction of hazardous substances in non-food applications | Not generally applicable unless specified by end-market |
Bapolene 610P is therefore positioned in film structures where the converter values lower seal initiation temperature, high dart drop impact at reduced gauge, and improved optical clarity over conventional C4 Ziegler-Natta LLDPE. The material is not a drop-in replacement on every line; lower melt strength, higher viscosity sensitivity, and different bubble stability require verification on the target blown-film or cast-film asset. Extrusion trials should include die pressure recording, melt temperature profiling, bubble stability observation, full-thickness-map measurement, and seal performance testing before the resin is placed into uninterrupted production.