| HS Code | 284396 |
| Polymer Type | Low Density Polyethylene (LDPE) |
| Density | 0.922 g/cm³ |
| Melt Index | 2.0 g/10 min |
| Tensile Strength At Break Md | 24 MPa |
| Tensile Strength At Break Td | 22 MPa |
| Tensile Strength At Yield Md | 10 MPa |
| Elongation At Break Md | 500% |
| Elongation At Break Td | 600% |
| Dart Drop Impact | 120 g |
| Elmendorf Tear Strength Md | 200 g/mil |
| Elmendorf Tear Strength Td | 300 g/mil |
| Haze | 6% |
| Gloss | 80% |
| Melting Point | 110 °C |
| Vicat Softening Point | 95 °C |
| Coefficient Of Friction | 0.2 |
As an accredited Bamberger Polymers Bapolene® 2292 Polyethylene Film Grade factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Bamberger Polymers Bapolene® 2292 Polyethylene Film Grade comes in 25 kg polyethylene-lined bags, typically shipped on 1,000 kg pallets. |
| Container Loading (20′ FCL) | 20′ FCL loading of Bamberger Polymers Bapolene® 2292 Polyethylene Film Grade: palletized bags, securely stowed, dry container, weight-compliant, ambient temperature. |
| Shipping | Bamberger Polymers Bapolene® 2292 Polyethylene Film Grade is shipped as non-hazardous resin pellets, typically in 25 kg moisture-resistant bags on pallets or in bulk containers. Transport in clean, dry vehicles. Protect from heat, moisture, and sunlight; avoid ignition sources. Not DOT/IMDG/IATA regulated. Store cool and dry. |
| Storage | Store Bapolene® 2292 in a cool, dry, well-ventilated warehouse away from direct sunlight, heat, sparks, and open flames. Keep original containers sealed and palletized to prevent moisture, dust, and contamination. Avoid contact with strong oxidizing agents. Maintain moderate temperatures, protect from UV exposure, and rotate stock using first-in, first-out. Follow supplier SDS and local regulations. |
| Shelf Life | Shelf life is typically 24 months from manufacture when stored in original unopened packaging, cool, dry, ventilated, away from heat and sunlight. |
High-stalk bubble geometry on a grooved-feed single-screw extruder with 30:1 L/D and die diameter 250 mm represents one of the most direct downstream uses of Bapolene 2292. In a monolayer structure intended for dry food overwrap, the dry blend is commonly set at 70–80 wt% Bapolene 2292, 15–25 wt% LDPE with a melt index of 0.25–0.35 g/10 min per ASTM D1238-20, and 2–5 wt% slip/antiblock masterbatch, with active erucamide slip migration adjusted to produce a kinetic coefficient of friction of 0.20–0.35 when measured by ASTM D1894-14. The formulation ratio must not push LDPE above 30 wt% if the converter is targeting a dart drop of ≥200 g on 25 µm film per ASTM D1709-16ae1, because at that loading the bubble tends to lose high-stalk stability and machine-direction tear propagation increases. The line is typically operated at a melt temperature of 190–215°C, die gap 1.2–1.8 mm, blow-up ratio 2.8:1–3.5:1, and a frost-line height 400–700 mm above the die, with internal bubble cooling used to hold gauge variation below ±6% across the layflat. Terminal products include paperboard tray overwrap, bakery bag liners, frozen vegetable bags, and cereal pouch liners.
| Compliance boundary | Reference or test method | Conversion condition |
|---|---|---|
| US food contact for olefin polymers | FDA 21 CFR 177.1520 | Direct dry food contact under Conditions A–H as assigned by food type and use temperature |
| EU plastic food contact materials | EU Regulation (EU) No 10/2011 as amended by Regulation (EU) 2020/1245 | Overall migration limit 10 mg/dm²; simulant selection per Annex III |
| China food contact for plastics | GB 4806.7-2016 | Total migration 10 mg/dm²; specific migration limits by substance |
| EU article communication duty | REACH (EC) No 1907/2006 | SVHC declaration threshold 0.1% w/w |
Operational boundary: if post-industrial regrind above 15 wt% is fed back without melt filtration, white specks and gel counts increase on the inner surface of bakery bag liners and can trigger visual rejection by downstream form-fill-seal inspection systems.
Across multi-season greenhouse and silage harvesting operations, Bapolene 2292 enters agricultural film structures as the main structural layer at 80–90 wt%, with a C6 or C8 metallocene LLDPE at 5–12 wt% to retain dart impact after UV exposure, and a 3–6 wt% black or white HALS masterbatch whose active hindered amine stabilizer content is controlled at 0.2–0.8 wt% of total film. The applicable compliance framework for silage clamp covers and bale wrap substrate is EN 13206:2017, while accelerated weathering is verified under ISO 4892-2:2013 at 1,500–2,500 h depending on geographic solar loading. On a three-layer blown film line with die gap 1.6–2.2 mm and blow-up ratio 2.5:1–3.2:1, the outer layers are formulated to carry the UV package while the core remains unmodified Bapolene 2292, which preserves extensional modulus and limits premature creep in field-installed greenhouse cladding. Melt temperature is held between 200–230°C to disperse HALS without forming free-fall gel defects. Terminal product types include greenhouse cladding, silage clamp covers, bale wrap substrate, and black mulch film; pro-oxidant or oxo-degradable additives should not be combined with this formulation because they can compromise the weathering claims required by EN 13206:2017.
Before a heavy-duty sack line commits Bapolene 2292 to the core layer, the converter typically fixes the blend ratio at 60–75 wt% Bapolene 2292, 15–25 wt% metallocene LLDPE, and 10–15 wt% LDPE for bubble stability, with the outer layers receiving 2–4 wt% anti-slip masterbatch to maintain stacking friction in warehouse storage. The three-layer blown film line is configured with 30:1–35:1 L/D grooved-feed extruders, die diameter 300–450 mm, internal bubble cooling, and a collapsing frame that reduces crease formation before corona treatment on the print side. Compliance verification focuses on mechanical performance rather than food migration: dart drop for 150 µm film is measured by ASTM D1709-16ae1, Elmendorf tear by ASTM D1922-15, and tensile yield by ISO 527-3:2018, while REACH (EC) No 1907/2006 remains applicable for substance content declarations. Post-consumer recyclate can be incorporated at up to 25 wt% in the core layer if the sack converter verifies that dart drop remains above 800 g and that film thickness variation stays within ±8% on the layflat. Terminal products include sewn open-mouth sacks, pinch-bottom valve sacks, and laminated woven polypropylene outer layers where Bapolene 2292 serves as the sealant web.
In monolithic construction vapor barriers and underside concrete retarders, Bapolene 2292 is used at 85–100 wt% with carbon black masterbatch at 2–3 wt%; the carbon black dispersion is controlled by film surface rating under ISO 18553:2002, and melt temperature is held at 200–220°C to avoid charred agglomerates that create pinholes in 50–150 µm membranes. The downstream blown film process for this application runs at a die gap of 2.0–2.5 mm, blow-up ratio 2.0:1–2.5:1, and layflat width typically above 1,800 mm to reduce seam count under concrete slab placement. Water vapor transmission is tested by ASTM E96/E96M-20, tensile properties by ASTM D882-18, and puncture propagation by ASTM D1709-16ae1; published water vapor permeance for Bapolene 2292 at 100 µm is limited, so converter-run calibration against the project specification is required. Terminal product types include underslab vapor retarders, crawl-space liners, temporary containment liners, and sacrificial concrete curing covers. The operational boundary for this sector is regrind reincorporation: post-industrial trim above 20 wt% can raise gel counts and reduce puncture resistance below the specification for concrete aggregate abrasion.
Mailer converters that operate at 180–250 pouches/min on bottom-seal machines require a coextruded three-layer film in which Bapolene 2292 occupies 50–70 wt% of the core layer, white masterbatch 8–12 wt% in one skin layer, and black masterbatch 2–4 wt% in the opposite skin layer to produce the opaque white/black structure common in e-commerce mailer stock. The film is blown on a three-layer line with die gap 1.8–2.4 mm, blow-up ratio 2.8:1–3.5:1, and melt temperature 195–215°C, then slit and transferred to a bottom-seal line where seal initiation temperature is 105–120°C and seal strength is verified by ASTM F88/F88M-21 at ≥9 N/25 mm for 50 µm film. Packaging waste compliance is governed by EU Packaging and Packaging Waste Directive 94/62/EC with a combined heavy-metal limit of ≤100 ppm for lead, cadmium, mercury, and hexavalent chromium, while US state model legislation under CONEG/TPCH applies the same 100 ppm threshold. Surface slip is set to 0.15–0.25 kinetic COF by ASTM D1894-14 to avoid feed jams in automated polybag insertion equipment. Terminal product types include white/black e-commerce mailer bags, opaque document envelopes, garment shipping pouches, and tamper-evident return polybags.
Once the can-liner line moves beyond 150 m/min, Bapolene 2292 is typically blended at 65–80 wt% with 15–25 wt% post-industrial regrind and 5–10 wt% LDPE or metallocene LLDPE for dart impact; if post-consumer reclaim is substituted, the upper reclaim limit is 15 wt% unless a melt filter of 120–180 µm is installed ahead of the die head. The extrusion process for this application uses a single-layer blown film line with die gap 1.8–2.4 mm, blow-up ratio 2.5:1–3:1, frost-line height 300–600 mm, and output controlled to keep melt temperature between 190–220°C, because higher shear heating can produce detectable odour volatiles in low-thickness can liners. Mechanical verification is based on ASTM D1709-16ae1 for dart drop on 25–60 µm film, ASTM D1922-15 for Elmendorf tear, and ISO 527-3:2018 for tensile elongation at break, while REACH (EC) No 1907/2006 documentation is maintained for any recycled content. Terminal products include kitchen can liners, janitorial sacks, and office wastebasket liners. The operational boundary for this sector is anti-static additive loading: quaternary ammonium or ethoxylated amine anti-stats above 0.5 wt% can lower heat-seal strength at the bottom-seal fold and should be avoided when the can liner is sealed on high-speed bag machines with jaw dwell times below 0.4 s.
Competitive Bamberger Polymers Bapolene® 2292 Polyethylene Film Grade prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Bamberger Polymers Bapolene® 2292 is a high-molecular-weight high-density polyethylene film resin supplied in pellet form for blown film extrusion. The material occupies the high-molecular-weight segment of HDPE film resins, with a nominal density in the range 0.950–0.955 g/cm³ as measured under ISO 1183-1:2019 and a melt mass-flow rate below 0.20 g/10 min under ISO 1133-1:2022 at 190°C and 2.16 kg. These two properties position the product for thin-gauge industrial liners, can liners, merchandise bags, and other blown film structures where stiffness, puncture resistance, and moisture-vapor barrier are required. Published data for this specific configuration is limited in open databases; the distributor’s technical data sheet and certificate of analysis control the exact additive package, molecular-weight distribution, and lot-specific values.
Under ASTM F1249-20 at 38°C and 90% RH, unmodified HMW-HDPE film at 25 µm thickness typically exhibits water-vapor transmission rates of 4–8 g/m²·day, lower than values for LLDPE of equivalent gauge. The density range corresponds to a crystalline fraction of roughly 65–80% when determined by differential scanning calorimetry under ISO 11357-3:2018. That crystallinity raises tensile modulus and reduces optical clarity compared with lower-density polyethylene; the high molecular weight of Bapolene 2292, however, increases chain entanglement and tie-molecule density, improving dart impact and environmental stress-crack resistance relative to medium-molecular-weight HDPE. The associated trade-off appears as higher extruder head pressure and reduced melt index, not as a loss of melt strength.
Weight-average molar mass for HMW-HDPE film resins generally falls between 150,000 and 300,000 g/mol as determined by gel permeation chromatography. The broad molar mass distribution contributes to die swell and bubble stability. Under ASTM D1709-16ae1 Method A, commercial HMW-HDPE film at 25 µm gauge commonly exceeds 300 g dart impact, and some grades reach 500 g or higher. Tensile properties measured under ISO 527-3:2018 at 500 mm/min for HMW-HDPE film typically show yield strengths of 22–30 MPa in the machine direction and elongation at break above 500%. Elmendorf tear measured under ASTM D1922-15(2020) is strongly anisotropic in HDPE film; transverse-direction tear often exceeds machine-direction tear by a factor of 5–15 because orientation and crystalline morphology dominate the propagation path.
Environmental stress-crack resistance, measured by ASTM D1693-15 Condition B, is generally higher for HMW-HDPE than for medium-molecular-weight HDPE because long chains form more tie molecules between lamellae. Published data for Bapolene 2292 under this specific configuration is limited, but the high-molecular-weight class is selected for contact with surfactants and light aliphatic hydrocarbons where standard HDPE grades fail. The molecular architecture also raises shear viscosity; therefore, processing equipment must be selected to deliver sufficient shear heating without exceeding the oxidation threshold.
| Property | Test method | Class range | Notes |
|---|---|---|---|
| Density | ISO 1183-1:2019 | 0.950–0.955 g/cm³ | Higher density raises modulus and moisture barrier |
| Melt mass-flow rate | ISO 1133-1:2022, 190°C, 2.16 kg | 0.05–0.20 g/10 min | Lower values indicate higher molecular weight |
| Dart impact | ASTM D1709-16ae1 Method A | 250–500 g at 25 µm | Gauge and blow-up ratio shift values |
| Tensile yield | ISO 527-3:2018 | 22–30 MPa | Machine direction |
| Elongation at break | ISO 527-3:2018 | 500–800% | Direction-dependent |
| Elmendorf tear | ASTM D1922-15(2020) | MD 15–35 g; TD 150–300 g | Anisotropic orientation |
| Water-vapor transmission | ASTM F1249-20 | 4–8 g/m²·day at 25 µm, 38°C, 90% RH | Lower than LLDPE |
In blown film production on monolayer lines with screw diameters of 45–90 mm and length-to-diameter ratios of 24:1–33:1, Bapolene 2292 is processed with a barrier screw or a high-shear mixing section to generate a homogeneous melt at head pressures typically between 25 and 45 MPa. Die gaps are set at 1.5–2.5 mm for HMW-HDPE, wider than the 0.8–1.2 mm gaps used for LDPE, because the higher molecular weight resin produces higher die swell and melt-fracture risk. Blow-up ratios are commonly 3:1–5:1, with frostline heights maintained at 6–10 die diameters; bubble stability at these settings depends on melt strength, and excessive blow-up ratio above 5:1 can induce periodic bubble sag followed by thickness spikes. Melt temperature at the die is usually controlled between 190°C and 230°C; excursions above 260°C accelerate thermo-oxidative degradation and increase gel formation in the film.
Polyethylene film grades are generally stabilized with a hindered phenolic primary antioxidant and a phosphite secondary antioxidant; Bapolene 2292 may contain a neutralizer and, depending on the distributor’s order configuration, a slip or antiblock additive. The exact additive formulation must be obtained from the technical data sheet because it affects coefficient of friction under ASTM D1894-14 and blocking force under ASTM D3354-15. For food-contact applications, unmodified polyethylene homopolymer can meet FDA 21 CFR 177.1520(c) when the film is used in accordance with the specified extractives limitations; the specific Bapolene 2292 lot should be verified against the manufacturer’s food-contact statement. Under European food-contact legislation, compliance with Regulation (EU) 10/2011 requires migration testing under the intended food simulant, time, and temperature conditions; no blanket food-contact approval applies without such testing.
For industrial packaging, the resin is generally outside the scope of REACH registration restrictions as a polymer; however, imported compounds may require confirmation that monomer and additive residues meet the relevant thresholds. The grade is not formulated with cadmium, lead, mercury, or hexavalent chromium above limits in Directive 2011/65/EU (RoHS), but the final film is not considered an electrical or electronic component unless converted for such use.
| Document | Condition | Requirement |
|---|---|---|
| FDA 21 CFR 177.1520(c) | Food-contact film | Homopolymer polyethylene; extractive limitations |
| Regulation (EU) 10/2011 | Food-contact migration | Overall migration below 10 mg/dm² unless stated otherwise |
| REACH | EU market | SVHC content below 0.1% w/w per article |
| Directive 2011/65/EU | Electrical/electronic film | Pb, Cd, Hg, Cr(VI), PBB, PBDE limits |
Compared with butene-LLDPE film resins, Bapolene 2292 produces film with higher tensile modulus and lower water-vapor transmission, but measurably lower clarity. Haze values under ASTM D1003-13(2021) for HMW-HDPE film frequently exceed 30%, whereas LLDPE blown film can fall below 10%. The higher density also raises seal initiation temperature; HDPE film typically requires seal temperatures above 135°C under ASTM F2029-16(2021), while LLDPE seals near 100–110°C. In applications where optical appearance or low-temperature sealing is critical, Bapolene 2292 is therefore not a direct drop-in replacement for LLDPE without equipment and downstream sealing adjustments.
Unlike high-pressure LDPE, Bapolene 2292 lacks long-chain branching and exhibits less strain hardening in extension. Its melt strength is achieved primarily through high molecular weight and chain entanglements, not long-chain branching. On coextrusion lines, Bapolene 2292 is commonly placed in the core or core-side layers of five-layer films rather than in the seal layer, because the seal layer demands a lower-melting resin such as LLDPE or LDPE. This structural difference also means that bubble stability on air-cooled blown film lines is more sensitive to die-lip shear stress and melt-temperature uniformity than is the case for LDPE-rich structures.
Operational limits arise when screen packs, melt pipes, or die gaps are sized for lower-viscosity polyethylene. Sustained head pressure above 45 MPa indicates either excessive screw speed, insufficient melt temperature, screen-pack blinding, or a die gap too narrow for the viscosity of HMW-HDPE. The failure mode observed on production lines is usually melt fracture at the die lip, visible as sharkskin or orange-peel surface roughness, followed by reduced tear resistance and gauge variability. Melt fracture in HMW-HDPE can be mitigated by raising melt temperature within the 200–230°C range, increasing die gap, or adding a fluoropolymer processing aid at 200–800 ppm; the processing aid coats die-lip metal and reduces shear stress, but its use must be disclosed if the film is intended for direct food contact.
If the resin is stored outdoors in humid conditions, surface condensation should be removed before processing. Polyethylene has negligible equilibrium moisture absorption; however, free surface water entering the feed throat can cause surging and bubble instability. A hopper dryer set at 60–70°C for 1–2 h is adequate for surface moisture removal, but prolonged drying above 90°C can soften pellets and cause bridging in the hopper. The resin should not be dry-blended with polypropylene or polyamide because phase separation produces delamination in the film; coextrusion with a tie layer is required if barrier polymers are combined with Bapolene 2292 in a multilayer structure.
In industrial liner applications where the film is filled at rates above 20 bags/min on vertical form-fill-seal machines, the combination of HMW-HDPE stiffness and tear resistance permits gauge reduction relative to LLDPE; however, the higher seal initiation temperature requires longer dwell times or higher jaw temperatures. Blown film lines converting Bapolene 2292 must therefore maintain stable bubble geometry and tightly controlled melt temperature to avoid seal contamination from gel particles generated by oxidative degradation at excessive temperatures.