| HS Code | 978053 |
| Polymer Type | Polyethylene, Injection Grade |
| Density | 0.952 g/cm3 |
| Melt Flow Rate 190 C 2 16 Kg | 5.0 g/10 min |
| Tensile Strength At Yield | 23.0 MPa |
| Tensile Elongation At Break | 800% |
| Flexural Modulus | 1.00 GPa |
| Notched Izod Impact | 0.500 J/cm |
| Hardness Shore D | 65 |
| Deflection Temperature At 0 45 Mpa | 70.0 °C |
| Vicat Softening Point | 126 °C |
| Linear Mold Shrinkage | 0.020-0.025 cm/cm |
| Water Absorption | 0.010% |
As an accredited Bamberger Polymers Bapolene® 2272 Polyethylene, Injection Grade factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Bapolene® 2272 polyethylene injection grade is supplied in 25 kg (55 lb) bags, 40 bags per pallet (1,000 kg). |
| Container Loading (20′ FCL) | Bamberger Polymers Bapolene® 2272 Polyethylene, Injection Grade: 20′ FCL, 25 kg bags, palletized/stretch-wrapped; approx. 18–22 MT per container. |
| Shipping | Shipping description: Bamberger Polymers Bapolene® 2272 Polyethylene, Injection Grade is a non-hazardous, non-regulated solid polymer. It is typically shipped in 25 kg bags, gaylords, or bulk trucks/railcars. Store dry, away from heat, moisture, and contamination. No special DOT, IMDG, or IATA shipping requirements apply. Handle with care to prevent bag damage and spillage. |
| Storage | Store Bapolene® 2272 polyethylene resin in a cool, dry, well-ventilated area away from direct sunlight, heat, sparks, and flames. Keep original containers closed to prevent moisture, dust, and contamination. Use pallets, avoid floor contact, and practice FIFO. Maintain moderate temperatures, avoid oxidizing agents, and ensure good housekeeping to prevent slip hazards from spilled pellets. |
| Shelf Life | Shelf life is 12 months when stored in original unopened packaging in a cool, dry place, away from direct sunlight. |
Injection molding of returnable transport packaging with Bapolene® 2272 is run as a high-flow HDPE system in the 20–30 g/10 min melt-index band. Side-wall sections are held to 2.0–3.5 mm, rib-to-wall ratios to 0.5–0.7, and untextured core-face draft angles to 0.5–1.5°. General-purpose reciprocating screws with L/D ratios of 20:1–24:1 and compression ratios of 2.5:1 are used. Melt temperature is maintained at 210–240 °C, mold temperature at 10–30 °C, and back pressure at 0.5–1.5 MPa. Injection velocity is profiled from 150 mm/s to 250 mm/s, while holding pressure is staged at 40–70 MPa. Cavity pressure sensors at the gate read 45–60 MPa during pack-and-hold. On 1,200 t toggle-clamp presses running 48-cavity pallet-foot tools, cooling time is controlled by thick boss sections: a 6 mm nominal diameter boss commonly requires 12–20 s additional hold before ejection without gate stringing.
For outdoor crates and totes, 0.2–0.5 wt% hindered amine light stabilizer and 1.5–2.5 wt% carbon black are dry-blended in a tumble mixer. The stabilizer package is selected against ISO 4892-2 cycle A weathering exposure. When the pigment and stabilizer carriers are olefin-based, the system retains compliance with FDA 21 CFR 177.1520 for incidental food contact. Mechanical acceptance commonly references tensile yield of 23–29 MPa per ASTM D638-14, flexural modulus of 900–1300 MPa per ASTM D790-17, and notched Izod impact of 2–4 kJ/m² per ISO 180/A. Deflection temperature under load for unfilled HDPE in this density band is typically 65–80 °C at 0.455 MPa per ASTM D648-18. Melt temperature above 260 °C should be avoided because molecular weight loss accelerates and can cause plate-out on core pins. Prolonged exposure to chlorinated cleaning agents at elevated temperature is not recommended; the high melt index that benefits rib filling reduces environmental stress-crack resistance relative to blow-molding HDPE grades.
Low-temperature impact response in thin-wall HDPE dairy containers is governed by wall thickness, processing-induced orientation, and spherulite size control. Bapolene® 2272 is processed in 0.8–1.5 mm wall sections with melt temperatures of 220–245 °C and mold temperatures of 15–25 °C. Fill time is set at 0.20–0.35 s, with a 0.05–0.10 s decompression stroke after screw recovery to reduce gate frost in cold-runner sub-gates. Peak cavity pressure should reach 45–70 MPa during filling to maintain density in rim and base vertices. If mold temperature falls below 15 °C, ductile-to-brittle transition shifts to warmer temperatures and freezer impact failure occurs at the base corner. High-cavitation molds with 32–48 cavities require hot-runner manifold temperatures of 230–250 °C; gate diameter should not exceed 0.8 mm to avoid gate stringing.
The resin is normally fed as 100% virgin high-flow HDPE. If notched Izod impact at −20 °C must exceed 3 kJ/m² per ISO 180/A, up to 5 wt% of a metallocene-catalyzed LLDPE with density below 0.920 g/cm³ is dry-blended. This addition raises low-temperature notched Izod by 10–25% but reduces flexural modulus by 8–15%; rib depth is reduced by 0.2–0.5 mm to preserve stacking stiffness. Migration testing under EU 10/2011 for repeated-use containers and cold-fill conditions is run after screw homogenization, because inadequate mixing can cause weld-line streaks and variable total migration. Published data for Bapolene® 2272 in freezer-grade dairy container configurations is limited; the processing window is derived from high-flow HDPE of equivalent melt-index class and should be validated on the actual production tool.
Caps and closures molded from Bapolene® 2272 concentrate dimensional tolerance in the sealing lip, tamper-evident band rupture points, and internal thread root. In a 28 mm PCO 1881 closure, roundness is held to ±0.10 mm and tamper-evident bridge length is held to 0.25–0.35 mm at the parting line. High-cavitation closure tools with 32–64 cavities are run at melt temperatures of 225–250 °C and mold temperatures of 10–20 °C. Valve-gated hot runners with 0.6–0.8 mm gate orifices produce gate vestige below 0.10 mm when decompression is set to 0.5–1.0 mm. On 130 t tie-bar-less molding machines, the limiting constraint is not injection speed but cooling uniformity across the cavity bank; a mold temperature variation of 3 °C between cavities can change removal torque by more than 5%.
Torque retention is influenced by thread-core creep and sealing-liner recovery. The resin is processed without filler; oleamide may be added at 0.05–0.10 wt% to reduce friction during induction sealing. Closures for aqueous, acidic, and low-alcohol food contact are tested under FDA 21 CFR 177.1520(c) and EU 10/2011. For household chemical bottle closures, stress-crack resistance is evaluated under ASTM D1693-15 condition B in a 10% Igepal CO-630 solution at 50 °C. Melt temperature above 255 °C during color changes should be avoided because degradation residues accumulate on hot-runner tips and cause gate stringing. Published data for Bapolene® 2272 in beverage closure torque retention is limited; liner compression can override the resin contribution and must be validated on the specific induction-sealed liner.
Injection molded open-head pails require rim hoop strength and handle boss load transfer without stress whitening. Bapolene® 2272 is applied in pails with nominal rim thickness of 2.5–4.0 mm and handle boss diameter of 16–20 mm. Melt temperature is set at 215–235 °C, while rim and boss mold temperatures are maintained at 20–30 °C to control post-mold ovality. Packing pressure is profiled at 55–75 MPa for 4–8 s, followed by cooling of 20–35 s depending on floor thickness. On a 650 t hydraulic press running a 4-cavity pail mold, handle boss voids are eliminated by reducing injection velocity at the boss transition to 80–120 mm/s and applying a short decompression after screw recovery. Shrinkage after 48 h at 23 °C and 50% RH is typically 1.5–2.0% in rim diameter for HDPE of this density class.
Pails intended for dangerous goods are evaluated under 49 CFR 178.601 or UN Model Regulations performance tests, including stacking at 40 °C for 28 days. High-flow injection HDPE may show lower environmental stress-crack resistance than high-molecular-weight HDPE used in blow-molded pails; open-head pails exposed to aggressive hydrocarbons may require a liner or barrier layer. Industrial pails can be colored with carbon black at 1.0–2.0 wt% without affecting RoHS 2011/65/EU thresholds for lead, mercury, cadmium, hexavalent chromium, PBB, and PBDE when applicable. The table below summarizes the compliance matrix for injection molded pail applications.
| Standard or regulation | Test focus | Application condition for injection molded pails |
|---|---|---|
| FDA 21 CFR 177.1520(c) | Olefin polymers for food contact | Applicable only to pails intended for direct food contact; migration depends on use conditions A through H. |
| EU 10/2011 | Overall and specific migration | Repeated-use pails with cold-fill or ambient storage; overall migration limit 10 mg/dm². |
| 49 CFR 178.601 | UN performance testing | Stacking, drop, and leakproofness for dangerous goods pails; test limits depend on packaging group. |
| RoHS 2011/65/EU | Restricted substance thresholds | Applies only when the pail is a component in electrical or electronic equipment. |
Published data for Bapolene® 2272 in UN-certified pail configurations is limited; tooling validation should include load-deflection measurement on the handle boss after 24 h ambient conditioning and post-mold diameter measurement at 23 °C and 50% RH before release for stacking qualification.
Structural requirements shift from thin-wall fill to ribbed load-bearing floors. Bapolene® 2272 fills complex rib patterns at melt temperatures of 220–245 °C, but gate velocity above 300 mm/s can create jetting at the flow front. For bins with shot weights above 1.5 kg, screw-back speed is set at 60–100 rpm and nozzle decompression is limited to 0.5 mm to prevent air entrapment. Mold temperature is set at 20–30 °C. Floor sections of 4–6 mm require holding pressure of 60–80 MPa for 10–20 s to avoid sink marks at rib intersections. Ejection temperature should not exceed 55 °C to prevent distortion of unsupported floor panels.
For vented bins used in industrial logistics, the formulation may include 1.0–2.0 wt% carbon black and 0.3–0.8 wt% antioxidant package. Antistatic grades require an internal antistat at 0.5–1.5 wt%, which reduces surface resistivity to 10^9–10^11 Ω per IEC 61340-2-3 but may slightly lower flexural modulus. Dimensional tolerance for mating lids is held to ±0.25 mm across a 600 mm span, requiring uniform mold cooling and post-mold fixturing for 24 h at 23 °C. High-flow HDPE of this class has lower environmental stress-crack resistance than high-molecular-weight HDPE; bins exposed to aromatic solvents or concentrated detergent solutions may require compatibility testing before production release.
In multi-cavity toy tooling, parting-line deflection on small cores is the primary source of dimensional rejection rather than material shrinkage. Bapolene® 2272 is processed with melt temperatures of 215–235 °C and mold temperatures of 12–25 °C. For action figures with 1.5–2.5 mm wall sections, injection speed is profiled from 60 mm/s at the core pin to 180 mm/s at the torso cavity to reduce core shift. Pigment masterbatches are added at 1–3 wt%; dispersion is verified under ASTM D6290-19 on flat plaques. Compliance with EN 71-3, ASTM F963-17, and REACH Annex XVII is required for toy-grade material; because the base resin is an unplasticized polyethylene, phthalate migration risk is below the regulated limit when the pigment masterbatch is also phthalate-free.
The high-flow nature assists filling of thin limbs and undercuts but reduces melt strength for microfeature retention. Ejection temperature should not exceed 55 °C to prevent distortion of unsupported appendages. Shrinkage after 48 h at 23 °C and 50% RH is in the range of 1.2–2.0% for unfilled HDPE of this density band; mold cavities are cut with 1.4% isotropic shrink allowance. Published data for Bapolene® 2272 in toy-grade formulations is limited; the shrink allowance is based on equivalent high-flow HDPE grades and should be confirmed with a pilot cavity before full tooling is completed.
Competitive Bamberger Polymers Bapolene® 2272 Polyethylene, Injection Grade prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Bamberger Polymers Bapolene® 2272 is an injection-grade high-density polyethylene supplied as a pelletized resin for high-flow mold filling. Distributor technical data list a nominal melt flow rate of 22 g/10 min when tested at 190 °C under a 2.16 kg load in accordance with ASTM D1238-20, and a density of 0.956 g/cm³ determined by ASTM D1505. Typical published property ranges include a tensile yield strength between 25 MPa and 28 MPa under ASTM D638-14 Type IV at 50 mm/min, a flexural modulus from 1,000 MPa to 1,200 MPa by ASTM D790-17 Procedure A, and a notched Izod impact value of 50 J/m to 70 J/m at 23 °C per ASTM D256-10. The grade is positioned for thin-wall injection molding where melt flow above 15 g/10 min lowers filling pressure and permits longer flow lengths than intermediate-flow HDPE grades.
Because Bapolene 2272 is a high-flow HDPE, its melt elasticity is lower than that of fractional-melt resins, but its rapid crystallization and moderate density still produce measurable stiffness. The public technical summaries do not always disclose the comonomer type or the molecular weight distribution; capillary rheometry data across the shear-rate range typical of injection molding have not been published for this specific grade. Processors commonly estimate viscosity from the 22 g/10 min melt flow datum and from spiral-flow trials on production tooling. At shear rates above 10,000 s⁻¹, published data for this specific configuration is limited.
The melt flow rate is the primary differentiator. Intermediate-flow HDPE injection grades frequently run between 8 g/10 min and 10 g/10 min; they provide higher notched Izod impact but require higher injection pressure or wider flow channels. Fractional-melt HDPE grades below 1 g/10 min are generally unsuitable for thin-wall injection molding because their high melt strength and low flow produce short shots at gate shear rates below 1,000 s⁻¹. Bapolene 2272 reduces viscosity enough for multi-cavity filling but sacrifices some ambient notched impact resistance relative to lower-flow grades. The following table compares published property envelopes for these three classes.
| Property | Bapolene 2272 typical envelope | Intermediate-flow HDPE | Fractional-melt HDPE |
|---|---|---|---|
| Melt flow rate (ASTM D1238-20, 190 °C/2.16 kg) | 21–23 g/10 min | 8–10 g/10 min | 0.3–0.7 g/10 min |
| Density (ASTM D1505) | 0.955–0.957 g/cm³ | 0.954–0.958 g/cm³ | 0.953–0.957 g/cm³ |
| Tensile yield strength (ASTM D638-14) | 25–28 MPa | 26–30 MPa | 27–32 MPa |
| Flexural modulus (ASTM D790-17) | 1,000–1,200 MPa | 1,050–1,250 MPa | 1,200–1,450 MPa |
| Notched Izod impact (23 °C, ASTM D256-10) | 50–70 J/m | 60–80 J/m | 150–300 J/m |
| Typical mold shrink (ASTM D955-08) | 1.8–2.2 % | 2.0–2.5 % | 2.5–3.5 % |
At equal wall thickness, Bapolene 2272 requires lower filling pressure than a 8–10 g/10 min HDPE and shortens injection time. The trade-off appears in notched Izod impact: the 50–70 J/m envelope is below the 60–80 J/m typical of intermediate-flow grades and substantially below fractional-melt materials. For cold-chain packaging, the lower-flow grades are often preferred unless the design compensates with ribbing or increased wall section. Subambient impact testing is required before substitution.
On production-scale injection molding lines, Bapolene 2272 is processed without predrying when stored under dry conditions. If relative humidity exceeds 60 % and surface condensation is visible, a hopper dryer set at 70 °C to 80 °C for 1 h removes surface moisture. Barrel set temperatures from 200 °C to 240 °C are used, with the rear zone maintained 10 °C to 20 °C below the nozzle to stabilize the feed wedge. Mold temperatures from 10 °C to 40 °C reduce cooling time but increase residual stress and differential shrinkage at the lower end. Reciprocating screw machines with 20:1 to 24:1 L/D and compression ratios of 2.5:1 to 3.0:1 are standard. Back pressures of 50 bar to 100 bar homogenize melt temperature without excessive shear work; screw surface speeds above 0.3 m/s should be avoided at small screw diameters because high-flow HDPE is subject to viscous heating and discoloration.
Shot size should be maintained between 30 % and 70 % of barrel capacity; residence time below 5 min is typical to avoid molecular weight reduction. At shot sizes below 20 % of capacity, melt residence time increases and the narrow flow distribution of Bapolene 2272 can degrade, shifting the melt flow rate above the nominal 22 g/10 min. Injection speed is set by flow length and gate geometry; high-flow HDPE permits injection speeds of 100 mm/s to 250 mm/s in thin-wall tools, but excessive speed produces jetting and surface defects at the gate.
At processing temperatures, high-flow HDPE behaves as a pseudoplastic melt. The power-law index of injection-grade HDPE at 190 °C typically ranges from 0.3 to 0.5; the viscosity at 1,000 s⁻¹ for a 22 g/10 min HDPE is often below 100 Pa·s but the exact curve for Bapolene 2272 has not been published. This shear-thinning behavior reduces pressure drop through runners and gates, but it also reduces melt strength and can increase gate blush. Molders using sequential valve gating must set valve opening times according to flow-front position rather than timer alone to avoid knit lines in high-flow materials.
In thin-wall containers with nominal wall thickness 0.8 mm and flow lengths above 150 mm, gate pressure losses control fill. Valve-gated hot-runner systems with 0.8 mm to 1.2 mm gate diameters and gate lands below 0.5 mm prevent premature solidification and gate-stringing. Cavity pressure required to fill such parts typically ranges from 300 bar to 500 bar; clamp force calculations based on 3 kN/cm² to 5 kN/cm² of projected area are used. When clamp force is insufficient, the high-flow melt penetrates parting-line clearances below 0.02 mm and produces flash. Excessive clamp force on multi-cavity tools can deform venting lands; vents should be maintained at 0.01 mm to 0.03 mm depth for high-flow polyethylenes.
In thin-wall HDPE molding, cooling is often longer than filling. Bapolene 2272, with a density of 0.956 g/cm³, recrystallizes with a heat of fusion typical for HDPE, approximately 190–210 J/g by ISO 11357-3. For 0.8 mm walls molded at 20 °C steel temperature, freeze time may be 1–2 s, whereas 1.5 mm walls may require 4–6 s. Cooling-channel layout must maintain a temperature differential across the cavity surface below 5 °C; otherwise differential shrinkage alters part flatness. Published thermal diffusivity data for this specific grade are limited, but molders use transient heat-transfer formulas based on the thermal conductivity of HDPE class materials to estimate cycle time.
Cycle time estimation for high-flow HDPE follows the same solidification limit as lower-flow grades; the higher melt flow does not override thermal diffusivity. For a 1.0 mm wall thickness, the cooling time constant is roughly 0.4 s to 0.6 s per degree of temperature difference between melt and mold; total cooling time of 8 s to 12 s is common. The actual value depends on part thickness, mold steel conductivity, and cooling-channel placement. A mold with conformal cooling channels can reduce cooling time by 20 % to 30 % compared with conventional drilled channels, but the resin’s differential shrinkage remains.
Warpage in high-flow HDPE parts is driven by flow-induced orientation and variable cooling. The high melt flow of Bapolene 2272 allows lower filling pressure, but rapid cooling through the recrystallization range can freeze anisotropic shrinkage. The relevant measurement method is ASTM D955-08, which reports mold shrinkage parallel and perpendicular to flow. Typical mold shrinkage for Bapolene 2272 is 1.8 % to 2.2 %, with differences between parallel and perpendicular directions sometimes exceeding 0.2 percentage points. In long flat lids, mold designers typically relocate gates to reduce orientation mismatch.
Oxidative degradation in high-flow HDPE accelerates above 280 °C. Extended melt residence above this temperature increases gel formation or discoloration in Bapolene 2272; the visible effect is yellowing at the gate or streaks in the molded part. Production interruptions should be managed by reducing barrel temperatures in the rear zones and purging with a lower-viscosity HDPE or LLDPE with melt flow between 12 g/10 min and 20 g/10 min. The purge is complete when the melt stream is clear and hydraulic back pressure returns to the set point. The grade should not be combined with peroxide concentrates beyond levels specified for controlled rheology adjustment unless melt flow and gel-count testing are performed, because melt flow can rise above 30 g/10 min and reduce impact properties below the published envelope.
Application areas documented for high-flow HDPE injection grades include thin-wall food containers, dairy tubs, overcaps, toys, and housewares with snap-fit features. In food-contact thin-wall containers, the high MFR enables filling of radial-flow molds at reduced clamp force; however, final article performance must be tested for top-load and drop impact according to distribution-chain standards rather than resin properties alone. Published data for Bapolene 2272 in frozen-food containers is limited; substitution into cold-temperature applications requires validation using ASTM D746-20 brittleness temperature or instrumented impact testing on molded parts.
Compared with high-flow metallocene LLDPE injection grades with melt flow near 20 g/10 min, HDPE Bapolene 2272 has a higher flexural modulus and lower toughness; the LLDPE counterpart typically shows notched Izod values above 100 J/m but lower stiffness. In caps and closures, HDPE is selected for stress-crack resistance and dimensional stability, while LLDPE is selected where impact or hinge flexure dominates. This distinction is material class rather than a difference among HDPE grades; for processors currently using a 8 g/10 min HDPE, Bapolene 2272 often reduces pressure drop by 20 % to 30 % in thin-wall tools, but impact toughness decreases accordingly.
The food-contact status of Bapolene 2272 is governed by olefin polymer provisions in 21 CFR 177.1520(c), which specifies permissible end uses and temperature limits for high-density polyethylene. A manufacturer’s food-contact statement should be obtained for each lot because the regulation applies to the polymer as intended to be used; final articles must also comply with extractive limits under 21 CFR 177.1520(b). Under European food-contact legislation, compliance with Regulation (EU) No 10/2011 requires overall migration below 10 mg/dm² for plastics, with verification according to EN 1186-1 and testing in relevant food simulants.
| Regulatory framework | Test or clause | Typical HDPE threshold | Verification condition |
|---|---|---|---|
| FDA food contact | 21 CFR 177.1520(c) | Conforms as an olefin polymer | End-use temperature and food type restriction |
| EU food contact | Regulation (EU) No 10/2011 | Overall migration 10 mg/dm² | EN 1186-1 simulants |
| EU packaging metals | Directive 94/62/EC | 100 mg/kg sum of Pb, Cd, Hg, Cr(VI) | Packaging sample digestion |
| RoHS 2011/65/EU | Annex II | Pb 1000 mg/kg, Cd 100 mg/kg, Hg 1000 mg/kg | XRF or ICP-OES after digestion |
Under REACH EC 1907/2006, substances of very high concern listed in Annex XIV and restrictions in Annex XVII must be assessed in finished formulations. Bapolene 2272 as an unmodified polyethylene typically contains no intentionally added SVHCs above the 0.1 % w/w communication threshold, but distributors should provide a REACH statement for the specific grade and lot because catalyst residues and additive packages vary.
Lot-to-lot variance in Bapolene 2272 is evaluated by melt flow rate and density. Injection molders often monitor the melt flow after drying and the purge viscosity shift after color concentrate addition. If a color masterbatch increases the melt flow by more than 15 %, the gate freeze time and cushion may need adjustment. Ash content is typically below 0.05 % for unpigmented HDPE, but filled or colored formulations must be checked separately because inorganic pigments alter density and notched Izod impact.
For pharmaceutical packaging, the relevant pharmacopoeia chapters may require additional testing for extractables and leachables under USP 661.1 or Eur. Ph. 3.1.3 rather than resin certification alone. Bapolene 2272 is not supplied as a medical-grade resin; therefore, any pharmaceutical or medical-device application requires a dedicated change-control and regulatory file from the manufacturer or compounder.
The grade is not intended for applications requiring weld-line strength comparable to fractional-melt HDPE; at knit lines in thin-wall parts, the notched Izod impact value may fall by 20 % to 40 % relative to the unfilled material. Drying is not required for moisture absorption, but surface contamination from recycled regrind or external lubricants can alter melt temperature and screw recovery. For high-speed closures and thin-wall housewares, tool trials remain the definitive method because published data for this specific configuration is limited at gate shear rates above 10,000 s⁻¹.