| HS Code | 157453 |
| Polymer Type | Low Density Polyethylene (LDPE) |
| Density | 0.922 g/cm3 |
| Melt Index | 2.0 g/10 min (190°C/2.16 kg) |
| Tensile Strength At Break Md | 20.7 MPa |
| Tensile Strength At Break Td | 19.3 MPa |
| Elongation At Break Md | 500% |
| Elongation At Break Td | 600% |
| Dart Drop Impact | 120 g |
| Elmendorf Tear Strength Md | 200 g/mil |
| Elmendorf Tear Strength Td | 300 g/mil |
| Haze | 8% |
| Gloss | 60% |
| Coefficient Of Friction | 0.20 |
| Vicat Softening Point | 88°C |
| Melting Point | 110°C |
| Blocking Strength | 100 g |
As an accredited Bamberger Polymers Bapolene® 152F Polyethylene Film Grade factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Bamberger Polymers Bapolene® 152F Polyethylene Film Grade is supplied in 25 kg polyethylene-lined, multi-wall paper bags, palletized and shrink-wrapped for industrial shipment. |
| Container Loading (20′ FCL) | Container loading (20′ FCL): Bapolene® 152F polyethylene film grade, 25 kg bags, palletized, shrink-wrapped, forklift-loaded; about 18–20 MT per container. |
| Shipping | Bamberger Polymers Bapolene® 152F Polyethylene Film Grade is typically shipped as non-hazardous thermoplastic resin pellets in sealed bags, stacked on pallets and stretch-wrapped. Transport in clean, dry trucks or containers, protecting from moisture, heat, sunlight, and contamination. No special UN classification is required. |
| Storage | Store Bamberger Polymers Bapolene® 152F Polyethylene Film Grade in a cool, dry, well-ventilated warehouse, in original sealed packaging on pallets off the floor. Keep away from direct sunlight, heat, sparks, flames, and strong oxidizers. Protect from moisture, dust, and contamination. Maintain ambient temperature and humidity, avoid prolonged UV exposure, practice FIFO stock rotation, and do not stack beyond safe height. |
| Shelf Life | Stable under proper storage; no specific shelf life. Keep cool, dry, away from heat, sunlight, and moisture in sealed original packaging. |
In blown-film converting operations targeting direct food-contact packaging, Bapolene 152F Polyethylene Film Grade is run as a 100% virgin low-density polyethylene body and sealing layer within monolayer and coextruded structures. The resin’s published film-grade density envelope of 0.921–0.924 g/cm³ and melt flow index range of 1.8–2.2 g/10 min under ASTM D1238-20 at 190 °C/2.16 kg place it inside the processing window for thin-gauge tubular film. Finished packaging compliance is evaluated under FDA 21 CFR 177.1520(c) and EU Regulation 10/2011 Article 12, which imposes an overall migration limit of 10 mg/dm² and requires food simulant testing with ethanol 10% or isooctane when the film contacts aqueous or fatty foods above 40 °C. Formulation modification is limited to a 10–30 wt% let-down of C6-LLDPE where converters specify higher dart impact strength, plus 0.3–1.0 wt% slip masterbatch and 0.5–1.5 wt% antiblock masterbatch. Processing aid addition above 0.15 wt% is seldom required unless melt fracture appears at line output above 120 kg/h.
Extrusion is typically performed on a 60 mm single-screw extruder with 25:1–30:1 L/D and a barrier flighted screw, using barrel profile settings from 150 °C at the feed section to 180 °C at the adapter, with die-head pressure held below 350 bar. The annular die gap of 0.8–1.6 mm is combined with a blow-up ratio of 2.0:1–2.8:1 and a single-lip air ring plus internal bubble cooling, maintaining frost line height 400–700 mm above the die. At gauge 0.015 mm, melt temperature is kept below 190 °C; above this threshold surface oxidation raises gel formation and reduces heat seal strength under ASTM F88/F88M. Converters report gauge variation increases to ±8% when frost line height exceeds 700 mm, producing blocking and print skip in wound rolls. Terminal finished products include bread bags, bakery bags, self-service produce bags, frozen-food liners, and light-gauge hygiene strip bags.
Thin-gauge agricultural and silage film produced from Bapolene 152F is governed by EN 13206:2017 for round bale wrapping and by REACH 1907/2006 for the stabiliser package, with UV masterbatch addition typically 0.5–1.5 wt% and IR absorber addition 0.2–0.8 wt% where tunnel greenhouse thermal retention is specified. At 0.015 mm, bubble breathing is initiated by insufficient melt strength once die gap falls below 1.0 mm and blow-up ratio exceeds 3.0:1; the frost line then oscillates between 2.5:1 and 3.5:1 at frequencies of 0.2–0.5 Hz, producing gauge bands of ±10% and reducing puncture resistance measured under ASTM D5748. The bubble instability is amplified by high-stalk cooling because the extended melt web above the die acts as a viscoelastic column with low bending stiffness at molecular weight distribution values typical for film-grade LDPE.
The corrective operating condition on production-scale lines is a 250 mm annular die with internal bubble cooling and a dual-lip air ring, melt temperature reduced to 155–170 °C, and frost line height raised to 700–1,000 mm. The formulation is held at 70–90 wt% Bapolene 152F with 10–30 wt% C4-LLDPE to increase melt extensibility without sacrificing draw-down. If the LDPE fraction exceeds 90 wt%, gauge uniformity below 0.020 mm degrades on extrusion lines running above 180 kg/h; if the LLDPE fraction exceeds 30 wt%, film stiffness and high-temperature dimensional stability decline. Output is limited by the air-ring heat transfer coefficient rather than screw capacity, and frost line deviation of ±50 mm is the practical control margin before bubble contact with the collapsing frame. Terminal products include silage bale wrap, greenhouse tunnel covers, floating row covers, and nursery overwintering envelopes.
For lamination converters handling coffee, snack, and medical flat pouches, a 20–60 µm Bapolene 152F sealant web is produced by blown film and subsequently laminated to 12 µm BOPET, 20 µm BOPP, or 7 µm aluminium foil. Compliance is evaluated under EU Regulation 10/2011 Article 12 at 10 mg/dm² total migration, FDA 21 CFR 177.1520(c), and ISO 11607-1:2019 where the converted pouch functions as a terminally sealed medical packaging sealant layer. Adhesive coat weight is held at 1.5–3.5 g/m² for solventless polyurethane systems, and corona treatment is adjusted to 38–42 dyn/cm before lamination; below 38 dyn/cm, dry peel strength under ASTM F88/F88M drops below 2.5 N/15 mm on aluminium foil at 50 µm sealant gauge. The sealant web is oriented at blow-up ratio 1.8:1–2.4:1 with die gap 0.8–1.2 mm and melt temperature 160–175 °C, wound at 25–40 N/linear m to prevent blocking.
The lamination line runs at 150–250 m/min with nip temperature 40–50 °C; hot-tack is optimised by adding 10–20 wt% metallocene-LLDPE where vertical form-fill-seal lines exceed 80 packs/min. The LDPE sealant must not be specified as the sole seal layer in retort pouches above 121 °C or in high-acid hot-fill above 95 °C because seal integrity degrades and interfacial delamination occurs at foil edges. Published data for this specific sealant configuration is limited; converters should validate seal strength and migration on the exact laminate gauge before releasing production. Terminal finished products include coffee brick packs, snack sachets, aroma-barrier trial packs, and medical flat pouches.
| Food-contact blown film | FDA 21 CFR 177.1520(c) | Olefin polymer specification | 10 mg/dm² total migration |
| Agricultural bale wrap | EN 13206:2017 | Bale wrap mechanical durability | Puncture resistance per ASTM D5748 |
| Laminated sealant web | EU 10/2011 | Article 12 overall migration | 10 mg/dm² |
| Construction sheeting | ASTM D4397-22 | Thickness and physical requirement | 0.15 mm minimum typical |
| Post-industrial regrind | ISO 14021:2016 | Recycled content claim verification | 15–30 wt% regrind |
| Collation shrink film | ASTM D2732-20 | Free shrink measurement | BUR 2.8:1–3.5:1 |
Unsupported blown film used in construction and industrial containment is converted at 100% Bapolene 152F with a carbon black masterbatch loading of 2.0–3.0 wt% and, where outdoor exposure exceeds 24 months, 0.5–1.0 wt% hindered-amine stabiliser masterbatch. The governing specification is ASTM D4397-22 for polyethylene sheeting, and water vapour transmission is certified under ASTM E96/E96M-22, typically 0.5–1.0 g/(m²·24 h) at 0.15 mm thickness and 23 °C/50% RH. Flame-retardant grades, when specified, incorporate 5.0–8.0 wt% brominated or intumescent concentrate; however, this modification reduces Elmendorf tear strength under ASTM D1922 by 20–30% and must be evaluated before use in tensioned enclosure films.
Extrusion is carried out on a 90 mm smooth-bore extruder with 30:1 L/D, die gap 1.2–2.0 mm, blow-up ratio 1.8:1–2.5:1, and melt temperature 165–185 °C; output is 250–350 kg/h for 0.15–0.25 mm film. Gusseted tube and slit sheeting are produced in widths up to 3,000 mm, and winding tension is controlled between 40–60 N/linear m to prevent edge-wrinkle winding defects. Terminal products include temporary building enclosures, crawl-space vapour retarders, concrete curing blankets, containment liners for drum storage, and equipment overwrap.
Post-industrial edge trim, start-up purge, and roll-end scrap recovered from Bapolene 152F converting lines can be reintroduced as regrind at 15–30 wt% in non-food industrial film. Self-declared recycled content claims must follow ISO 14021:2016, and food-contact use is permissible only when the recovered feedstock originates from the same compliant film and is recompounded under a validated quality system; post-consumer reclaim is excluded from direct food-contact structures unless a dedicated decontamination process is installed. Above 30 wt% regrind, converters on 90 mm extruders with 30:1 L/D observe gel count increase, dart impact variability above ±15% under ASTM D1709-22, and melt pressure oscillation exceeding 2.5 bar at constant screw speed.
Regrind is ground through a 6 mm screen, densified, and fed by a gravimetric side-feeder at 15–30 wt%; a continuous melt filter with 150–200 µm screen pack is fitted between the extruder and the die to remove char and crosslinked particulate. Processing temperatures are held in the 170–185 °C range to minimise oxidative chain scission, and a reprocessing stabiliser masterbatch is added at 0.1–0.3 wt% when multiple heat histories are anticipated. Terminal products include bin liners, industrial refuse sacks, automotive seat cover wrap, and non-food stretch collation overwrap.
Collation shrink and case overwrap converting uses Bapolene 152F as the base polymer blended with 20–40 wt% EVA copolymer of 9–14% vinyl acetate content to shift shrinkage onset and increase free shrink under ASTM D2732-20. The addition ratio is constrained because EVA above 40 wt% lowers modulus and raises blocking in wound rolls, while EVA below 20 wt% produces insufficient shrink force to hold irregular multipack geometries at line speeds above 30 packs/min. The process demands a high-stalk bubble with blow-up ratio 2.8:1–3.5:1, die gap 1.0–1.4 mm, and melt temperature 150–170 °C so that trapped biaxial orientation is retained until the film enters the shrink tunnel at 120–140 °C. A slip/antiblock masterbatch at 0.5–1.2 wt% controls coefficient of friction below 0.30 under ASTM D1894-14.
On a 70 mm extruder with 28:1 L/D, the frost line is positioned at 900–1,200 mm above the die, and the bubble is quenched at 12–18 °C to maximise orientation without bubble flutter. Terminal products include beverage can collation film, boxed-product overwrap, industrial bundling film, and printed multipack shrink sleeves where shrink force must not exceed the compression strength of the outermost package.
Competitive Bamberger Polymers Bapolene® 152F Polyethylene Film Grade prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Bapolene® 152F is a polyethylene film-grade resin supplied by Bamberger Polymers and classified in the high-pressure low-density polyethylene segment. The resin is therefore distinguished by long-chain branching, a broad molecular-weight distribution, and film-extrusion rheology. Its published melt index is 2.0 g/10 min when tested according to ASTM D1238-20 Procedure A at 190 °C under a 2.16 kg load, and its nominal density is 0.922 g/cm³ when tested according to ASTM D1505. These characteristics place it between lower-density autoclave LDPE film resins, which commonly fall below 0.920 g/cm³, and linear low-density polyethylene grades, which use short-chain branching rather than high-pressure long-chain branching for toughness. End uses reported for this resin class include garment bags, produce overwrap, general-purpose shipping film, and thin industrial liners. Product-specific film values such as dart impact, Elmendorf tear, haze, and coefficient of friction are not single-point material constants; they are affected by die gap, blow-up ratio, frost line height, and converter-added slip and antiblock masterbatches and should be obtained from lot-level certificates of analysis or production trials.
Bubble stability in blown film extrusion is controlled by melt strength, extensional strain hardening, air-ring velocity distribution, and die-land temperature uniformity. In Bapolene® 152F, the 2.0 g/10 min melt index reduces low-shear viscosity relative to 0.70–1.0 g/10 min film-grade LDPE, yet the high-pressure long-chain branching still produces strain hardening. On a 60 mm single-screw extruder with a 30:1 L/D barrier screw, a 120 mm spiral-mandrel die, and a dual-lip air ring, stable operation for this density/MI class is typically observed at blow-up ratios between 2.0 and 2.8, melt temperatures of 180–195 °C, die gaps of 0.8–1.1 mm, and frost line heights of 150–300 mm above the die face. At blow-up ratios exceeding 3.0, bubble flutter may appear unless internal bubble cooling is applied and the frost line is deliberately raised to dampen oscillation.
Bubble flutter at high blow-up ratios is frequently attributed to resin melt index; on production lines, it is more often caused by air-ring pressure imbalance, worn die lips, or a frost line position that is too low or too variable. A pressure difference greater than ±15% between quadrants of the air ring can induce cyclical thinning. Operators should record four-quadrant film thickness using a capacitance gauge or micrometer and compare the pattern to air-ring shim settings before changing resin. If the gauge band is uniform within ±5% but instability persists, the frost line should be raised or the melt temperature reduced by 5–10 °C. Because shear viscosity in this LDPE class is power-law with an index near 0.45–0.55, screw-speed increases from 20 rpm to 80 rpm do not increase motor load proportionally; however, above 90 rpm viscous dissipation can cause melt-temperature overshoot and die-lip drool. Melt temperature should therefore be monitored at the adapter rather than inferred from barrel set points.
Toughness can be monitored using dart impact according to ASTM D1709 Method A for film below 50 µm. The combination of 0.922 g/cm³ density and 2.0 g/10 min melt index generally places the grade in a general-purpose toughness range; downgauging below 25 µm should be validated on the target line because puncture and tear performance may decline below the acceptable specification.
Converters adding slip and antiblock masterbatches should record die pressure and screw recovery time before and after dosing. Masterbatch addition at 1–3 wt% can change viscosity only modestly but often lowers apparent melt temperature by introducing a lower-melting carrier resin. The final coefficient of friction should be measured according to ASTM D1894, not inferred from masterbatch loading alone. For films that require a low coefficient of friction, erucamide-based slip concentrates typically require 24–72 hours post-extrusion migration to reach equilibrium; coefficient of friction measured immediately after slitting will not represent final performance.
Pre-drying is not normally required when pellets are stored at ambient conditions below 60% relative humidity. Condensation on cold pellets should be avoided; if surface moisture is observed, drying at 55–65 °C for 2–4 hours in a desiccant dryer is sufficient. Melt residence time above 205 °C should be minimized for any high-pressure LDPE because prolonged thermal exposure can degrade long-chain branching and produce gel particles or odour. On cast film lines with a 45 mm extruder and a 250 mm slot die, melt temperatures above 195 °C may increase die-lip build-up, especially when the resin is run at high screw speed without adequate air-gap cooling.
| Parameter | Method or reference | Value or condition |
|---|---|---|
| Melt index | ASTM D1238-20 Procedure A | 2.0 g/10 min |
| Density | ASTM D1505 | 0.922 g/cm³ |
| Resin type | High-pressure LDPE film class | Long-chain branched, general-purpose |
| Food-contact suitability | FDA 21 CFR 177.1520(c) 2.1 or 3.1 | Lot-level supplier documentation required |
| EU food-contact status | Regulation (EU) No 10/2011 Annex I | Verify specific migration limits for intended food simulant |
| RoHS screening | Directive 2011/65/EU Annex II | Supplier declaration required |
Film property specifications such as tensile stress at break, elongation, dart impact, tear, haze, and gloss should be set by the converter and verified by ASTM D882, ASTM D1709, ASTM D1922, ASTM D1003, and ASTM D2457 on the actual extrusion line. Resin viscosity alone does not define finished-film property values. Published data for this specific configuration is limited; therefore, acceptance criteria should be generated from production-scale trials rather than from a generic datasheet.
Bapolene® 152F differs from higher-density polyethylene film grades because the lower density reduces stiffness and melting point; from lower-density LDPE grades because it improves modulus and film gauge economics; and from butene LLDPE because the high-pressure LDPE architecture gives higher die-lip melt strength and better shear thinning but lower dart impact and Elmendorf tear when compared at the same melt index. The substitution should be based on a requirement profile rather than on melt index alone.
In thin-gauge packaging, a change from a 0.918 g/cm³ high-pressure LDPE to Bapolene® 152F increases the density by 0.004 g/cm³. This raises secant modulus at 2% strain as measured by ASTM D882 and reduces theoretical yield area per unit mass; the film becomes slightly stiffer at equal gauge. Because density is increased while melt index is 2.0 g/10 min, the converter may observe a narrower stable bubble window at high blow-up ratios than with a 0.25–0.30 g/10 min heavy-duty LDPE, but lower head pressure and greater throughput at fixed screw speed. Seal strength should be measured according to ASTM F88/F88M-21a over the intended temperature range, since density and additive migration influence heat seal initiation. Hot-bar sealing can be evaluated with dwell times of 0.3–0.8 s and jaw pressures of 2–4 bar; the resulting seal strength depends on film thickness and seal-bar alignment.
Compared with butene LLDPE films, Bapolene® 152F typically has a more pronounced shear-thinning response and higher die-lip melt strength, which can improve bubble stability and reduce neck-in on cast lines. However, linear LLDPE grades of similar melt index usually display higher dart impact and machine-direction tear resistance by ASTM D1922; therefore this grade is not a direct replacement for LLDPE in heavy-duty, puncture-dominated packaging. Published data for this specific configuration is limited; where load retention or stretch force is critical, the converter should run side-by-side trials on the target line.
Storage and handling boundaries include avoiding dusty environments, avoiding polymer segregation with dissimilar melt-index regrind, and controlling regrind levels below 20 wt% when optical or seal consistency is critical. Higher regrind levels tend to increase gel contamination and lower dart impact. For coextruded structures, the resin may be used in core or seal layers; layer ratio and die construction should be matched to avoid interfacial instability between LDPE and lower-viscosity tie layers. If the application requires high puncture resistance, a butene or octene LLDPE with a density near 0.916–0.920 g/cm³ may be more appropriate; if the application requires melt strength and ease of processing, Bapolene® 152F remains within the general-purpose LDPE film class.