| HS Code | 591199 |
| Polymer Type | Low Density Polyethylene (LDPE) |
| Density | 0.922 g/cm³ |
| Melt Index | 2.0 g/10 min |
| Tensile Strength At Break | 2200 psi |
| Tensile Strength At Yield | 1400 psi |
| Elongation At Break | 600% |
| Dart Drop Impact | 100 g |
| Elmendorf Tear Strength Md | 300 g |
| Elmendorf Tear Strength Td | 400 g |
| Haze | 8% |
| Gloss | 70% |
| Coefficient Of Friction | 0.2 |
| Vicat Softening Point | 190 °F |
| Melting Point | 230 °F |
As an accredited Bamberger Polymers Bapolene® 152A Polyethylene Film Grade factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | Bamberger Polymers Bapolene® 152A Polyethylene Film Grade is packaged in 25 kg (55 lb) polyethylene bags, palletized for shipment. |
| Container Loading (20′ FCL) | Container loading for 20′ FCL: Bapolene® 152A polyethylene film grade in 25 kg bags, palletized, shrink-wrapped, and secured for ocean transport. |
| Shipping | Bapolene® 152A Polyethylene Film Grade is shipped as non-hazardous solid resin pellets in moisture-barrier bags, lined bulk bags, or bulk trucks/railcars. It is palletized and stretch-wrapped for dry van transport. Keep clean, dry, and away from heat and UV. No special DOT/IMDG/IATA dangerous goods classification. |
| Storage | Store Bamberger Polymers Bapolene® 152A Polyethylene Film Grade in a cool, dry, well-ventilated area, away from direct sunlight, heat, sparks, flames, and oxidizing agents. Keep containers tightly closed, palletized, and protected from moisture, dust, and physical damage. Maintain ambient temperature and use first-in, first-out stock rotation. Avoid prolonged excessive heat. Ensure good housekeeping to prevent slipping on spilled pellets. |
| Shelf Life | Bapolene 152A polyethylene film grade has a 24-month shelf life when stored cool, dry, and in original unopened packaging. |
Bapolene® 152A is processed as a primary food-contact blown film on single-screw extruders with screw L/D ratios between 25:1 and 30:1, barrel zones set between 150°C and 180°C, and adapter melt temperature verified by needle pyrometer at 170°C to 195°C. The die gap is held at 0.8 mm to 1.2 mm for film gauges between 20 µm and 60 µm, with a blow-up ratio of 2.0:1 to 2.5:1 and frost line position 5 to 8 die diameters above the die face. Erucamide slip masterbatch is metered at 1 wt% to 2 wt%, and synthetic silica antiblock masterbatch at 2 wt% to 3 wt%, via gravimetric feeders. Compliance for direct food contact is governed by FDA 21 CFR 177.1520(a)(2) with extractives controlled under (c)2.2, and by EU Regulation 10/2011 Annex I, where overall migration into food simulants must not exceed 10 mg/dm² for the finished article. Converters normally specify kinetic coefficient of friction below 0.30 after 72 h of additive bloom, measured by ASTM D1894, and haze below 7% at 50 µm, measured by ASTM D1003. End products include bread bags, produce bags, and frozen food liners where seal strength of at least 2.0 N/25 mm is confirmed by ASTM F88 at 130°C with 0.5 s dwell and 0.2 MPa jaw pressure.
Bapolene® 152A is used in transparent collation shrink film after dry blending with 10 wt% to 20 wt% of a butene-based linear low density polyethylene with melt index in the 0.8 g/10 min to 1.2 g/10 min range, measured by ISO 1133-1. The blend is processed on a blown film line equipped with internal bubble cooling at differential pressure of 0.5 kPa to 1.5 kPa and a dual-lip air ring. Blow-up ratio is raised to 3.5:1 to 4.5:1 to build transverse orientation, and the frost line is held 100 mm to 150 mm above the die with a tolerance of ±25 mm. Transverse shrink tension is measured in oil at 150°C by ASTM D2732, and converter specifications typically fall between 0.5 N/cm and 1.0 N/cm for can tray overwrap. The process window is narrow; ambient air velocity variations above 0.5 m/s across the bubble surface can initiate asymmetric strain hardening and gauge bands.
Increasing blow-up ratio above 4.0:1 does not produce a proportional gain in shrink tension because molecular orientation in the machine direction begins to relax when the film passes through the upper nip at lower line speeds. At these conditions, gauge variation must remain within ±8% of nominal thickness to prevent dog ears at the seal jaw and burn-through during hot-wire sealing. Seal initiation temperature of 152A-rich blends is measured by differential scanning calorimetry at 1°C/min and typically falls between 95°C and 105°C; lowering seal initiation below 90°C requires ethylene-vinyl acetate addition, which reduces shrink force at 150°C. End uses include beverage multipacks, canned goods tray overwrap, and office paper bundling. Published data for this specific configuration is limited when the processor uses water-quenched lower nip sets, so converter-run shrink tension checks are required before changing die geometry.
In three-layer coextruded greenhouse and silage covers, Bapolene® 152A is placed in the core layer at 40 wt% to 60 wt%, with skin layers formulated for anti-drip and ultraviolet resistance. Hindered amine light stabilisers are added at 0.20 wt% to 0.40 wt%, and a benzotriazole ultraviolet absorber at 0.10 wt% to 0.20 wt%, based on total film mass. Polymeric HALS grades are preferred over monomeric HALS to reduce migration to the outer surface, which causes whitening and rain wash-out. Die gap is set at 1.2 mm to 1.8 mm, blow-up ratio 2.5:1 to 3.0:1, and melt temperature 165°C to 190°C. Film thickness ranges from 150 µm to 200 µm for multi-season greenhouse cladding.
Accelerated weathering is conducted according to ISO 4892-2 cycle 1 or ASTM G154 cycle 1, with tensile elongation retention measured by ISO 527-3 after 4000 h of exposure. Retention criteria are set by the buyer and differ by geographic UV dose; published data for this specific configuration is limited for tropical high-UV sites. Processors should not exceed 200°C melt temperature because decomposition of the ultraviolet absorber raises free acidity and accelerates bubble instability. Compliance is checked against REACH Annex XVII entries for restricted phthalates and against EU 10/2011 if the film contacts silage intended for animal feed. End products include silage covers, greenhouse tunnel films, and low tunnel mulch where anti-drip additives are placed only in the inner skin to avoid interference with greenhouse condensate drainage.
| Application Segment | Standard or Regulation | Clause or Method | Requirement |
|---|---|---|---|
| Primary food contact | FDA 21 CFR 177.1520 | (a)(2), (c)2.2 | Olefin polymer extractives limits |
| Food contact film | EU 10/2011 | Annex I, overall migration | 10 mg/dm² or 60 mg/kg |
| Collation shrink film | ASTM D2732 | Oil immersion at 150°C | Shrink tension target by pack style |
| Greenhouse and silage film | ISO 4892-2 | Cycle 1 | Tensile retention per buyer specification |
| Heavy-duty construction liners | ASTM D1709 | Method A | Dart impact ≥ 400 g at 150 µm, converter-specific |
| Heavy-duty construction liners | REACH Annex XVII | Entries 50–52 | Phthalates < 0.1 wt% |
| Surface protection film | RoHS 2011/65/EU | Annex II | Pb, Hg, Cd, Cr6+, PBB, PBDE < 1000 ppm |
| Textile packaging film | AFIRM RSL 2024 | Apparel and footwear scope | Dimethylformamide, phthalates, organotins limits |
| Frozen food film | ASTM F88 | Seal strength method | ≥ 1.5 N/25 mm at 110–120°C |
For heavy-duty construction and demolition liners, Bapolene® 152A is blended with 15 wt% to 30 wt% linear low density polyethylene to meet ASTM D1709 Method A dart impact values above 400 g at 150 µm. The tubular film is produced with a die gap of 1.8 mm to 2.5 mm, a blow-up ratio of 1.8:1 to 2.4:1, and melt temperature 160°C to 185°C. Carbon black masterbatch is added at 2 wt% to 5 wt% for opacity and ultraviolet stability. On grooved-feed single-screw extruders with 30:1 L/D, throughput is limited by head pressure at 280 bar to 320 bar; screen packs above 80 mesh should be avoided because melt pressure rises toward the rupture disc setting. Regrind up to 30 wt% is usable in non-critical liners, but gel counts increase when regrind is stored in humid conditions. Pre-drying at 60°C for 2 h is required if ambient relative humidity exceeds 80%. End products include construction waste sacks, asbestos abatement liners, and moisture barriers under concrete. These films are not intended for food contact, and compliance focuses on REACH Annex XVII restrictions for restricted phthalates and polycyclic aromatic hydrocarbons in carbon black.
Surface protection films based on Bapolene® 152A are produced as two-layer coextruded structures in which the backing layer uses 152A and the cling layer contains 3 wt% to 6 wt% polyisobutylene with molecular weight in the 1,000 g/mol to 2,000 g/mol range. The cling layer accounts for 10% to 15% of total film thickness, which ranges from 30 µm to 70 µm. Peel adhesion to stainless steel is measured by ASTM D3330 at 180° and 300 mm/min; initial adhesion after 24 h typically falls between 0.4 N/cm and 0.8 N/cm, rising to 1.5 N/cm to 2.5 N/cm after 7 days at 23°C. Storage at 40°C accelerates tackifier migration and can produce adhesion build-up beyond the removal limit of 4.0 N/cm on painted surfaces. If the cling layer contains an amine-based slip additive, lacquer adhesion on re-coated steel can fail after film removal.
Processors use a melt temperature of 165°C to 190°C and a die gap of 0.8 mm to 1.0 mm, with blow-up ratio 2.0:1 to 2.8:1. Gel counts must stay below 10 per m² to avoid imprinting on polished stainless steel. Compliance for this application is checked against RoHS Directive 2011/65/EU Annex II for lead, mercury, cadmium, hexavalent chromium, PBB, and PBDE, all limited to 1,000 ppm, and against REACH candidate list SVHC content below 0.1 wt%. End uses include protection of stainless steel sheet, aluminum composite panels, glass, and automotive body panels.
At 20 µm to 35 µm gauge, textile and garment packaging film based on Bapolene® 152A is produced using high-stalk bubble geometry, with neck height 8 to 12 die diameters above the die. The high neck height develops balanced machine and transverse impact strength at low thickness. Antistatic masterbatch is metered at 0.05 wt% to 0.15 wt%; higher addition levels create surface exudation that changes friction and mars heat-seal consistency. Die gap is 0.6 mm to 0.8 mm, blow-up ratio 2.5:1 to 3.0:1, and melt temperature 160°C to 180°C. Gauge variation is maintained within ±4% for automated polybag machines. End products include garment polybags, mailer envelopes, and textile export packaging. Compliance is checked against the AFIRM RSL 2024 limits for dimethylformamide, phthalates, organotins, and perfluorinated compounds, and against REACH Annex XVII Entry 51 and Entry 52 for phthalate plasticisers below 0.1 wt% in plasticised articles.
For frozen food film at 40 µm to 80 µm gauge, Bapolene® 152A is used in monolayer and coextruded structures where tear propagation resistance after low-temperature conditioning is evaluated by ASTM D1922 after 24 h at -20°C. The amorphous fraction of low density polyethylene stiffens as the storage temperature approaches the glass transition range, so Elmendorf tear values measured at room temperature are not predictive of -20°C behaviour. Seal strength is tested by ASTM F88 at 110°C to 120°C, 0.3 s dwell, and 0.2 MPa jaw pressure, with minimum seal strength of 1.5 N/25 mm for frozen vegetable pouches. Die gap is 0.8 mm to 1.2 mm, blow-up ratio 2.2:1 to 2.6:1, and melt temperature 170°C to 195°C. Slip and antiblock levels are lower than in non-food films because the film must not dust onto frozen products. End products include IQF vegetable pouches, ice cream overwrap, and frozen meat interleaving film. Compliance follows FDA 21 CFR 177.1520 and EU 10/2011 when direct food contact is intended, with migration testing performed on the finished film rather than on resin powder.
Competitive Bamberger Polymers Bapolene® 152A Polyethylene Film Grade prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618005193850 or mail to sales8@ascent-chem.com.
We will respond to you as soon as possible.
Tel: +8618005193850
Email: sales8@ascent-chem.com
Flexible payment, competitive price, premium service - Inquire now!
Bapolene® 152A, distributed by Bamberger Polymers, is a low-density polyethylene film-extrusion resin whose reported nominal melt index is 1.5 g/10 min under ASTM D1238 conditions of 190°C and 2.16 kg piston load, with a nominal density of 0.922 g/cm³ by ASTM D1505. The product is a high-pressure LDPE grade; the resulting long-chain branching and broad molecular weight distribution distinguish it from linear-low-density polyethylene and fractional-melt LDPE. It is supplied in pellet form and is conventionally specified for blown-film applications that require moderate melt strength, acceptable optical quality, and stable bubble geometry on general-purpose extrusion lines. No drying is normally required for material taken directly from a dry storage bay. Additive packages such as slip, antiblock, and ultraviolet stabilizers are usually introduced as masterbatches at the feed throat rather than being incorporated at full commercial concentration in the base resin. The paragraphs below describe the grade’s specifications, processing behavior, comparative position, and operational limitations without assigning a universal ranking.
| Measurement | Test Method | Reported Nominal Value |
|---|---|---|
| Melt index | ASTM D1238 (190°C, 2.16 kg) | 1.5 g/10 min |
| Density | ASTM D1505 | 0.922 g/cm³ |
| Tensile yield strength, MD/TD | ASTM D882 | 10.5/10.0 MPa |
| Tensile break strength, MD/TD | ASTM D882 | 24/21 MPa |
| Elongation at break, MD/TD | ASTM D882 | 350/580% |
| Dart drop impact, F50 | ASTM D1709, 25 µm film | 85 g |
| Elmendorf tear, MD/TD | ASTM D1922 | 300/180 gf/25 µm |
| Haze | ASTM D1003 | 6.5% |
| Gloss at 45° | ASTM D2457 | 70 |
| Vicat softening point | ASTM D1525, 10 N | 94°C |
These values are typical for blown film of 25–50 µm gauge. They should not be read as specification limits; the seller’s certificate of analysis controls for a given lot. The melt index may also be expressed as melt flow rate under ISO 1133-1:2022; the result is nominally equivalent when the same temperature and load are used. The haze value of 6.5% at 25 µm should not be extrapolated to 75 µm film; haze scales roughly with thickness and surface roughness. The quoted gloss uses 45° geometry; values of 60 or below may still be acceptable for heavy-gauge liners but may be rejected for clear wrapping.
The distinction is most visible in melt index, long-chain branching content, and blown-film processing behavior. Fractional-melt LDPE grades with melt index in the 0.2–0.5 g/10 min range exhibit higher melt pressure and lower specific throughput on single-screw extruders, but they can support higher blow-up ratios and often yield higher dart impact in heavy-gauge films. Bapolene 152A, at 1.5 g/10 min, reduces screw pressure and permits higher output on underpowered lines; the trade-off is a reduction in bubble stability at very high blow-up ratios. C8-LLDPE film grades with similar melt index show higher tensile strength and puncture resistance because of linear chains and short-chain branching. However, linear architectures generate higher shear viscosity at the die lip and are more prone to sharkskin melt fracture unless die gaps are widened to 1.5–2.0 mm or processing aids are added. The long-chain branching in Bapolene 152A suppresses that particular instability and permits the use of conventional LDPE die gaps of 0.8–1.2 mm. For converters switching from LLDPE to LDPE, the main modification is a lower melt temperature profile and the possible elimination of fluoropolymer processing aid.
| Attribute | Bapolene 152A | Fractional-melt LDPE | C8-LLDPE |
|---|---|---|---|
| Melt index | 1.5 g/10 min | 0.2–0.5 g/10 min | 0.9–1.3 g/10 min |
| Density | 0.922 g/cm³ | 0.920–0.924 g/cm³ | 0.918–0.920 g/cm³ |
| Melt pressure on a 65 mm extruder at 20 kg/h | moderate | high | moderate to high |
| Bubble stability at 3.0:1 blow-up ratio | good | very good | line-dependent |
| Sharkskin resistance | good | good | poor without additives |
| Tensile strength | lower | lower | higher |
| Puncture resistance | lower | moderate | higher |
| Optical clarity | good | moderate | moderate to poor |
This qualitative comparison reflects general blown-film behavior, not a direct conversion between formulations; line-specific results depend on air-ring design, frost-line height, haul-off speed, and gauge control system. Converters should validate the comparison on the target equipment. On a production line equipped with a 100 mm grooved-feed extruder and 28:1 L/D screw, backpressure at 1.5 g/10 min is typically lower than for fractional-melt LDPE, but higher than for a 1.0 g/10 min LLDPE at equivalent output if no processing aid is used. The extruder drive amperage should be recorded during the first 4 h of production to establish a reference for screen pack condition. A rise in melt temperature without a corresponding rise in screw speed or barrel setpoint is often an early indicator of screw wear or distorted flow channels, not a change in the resin’s melt index.
On blown-film lines with a 65 mm single-screw extruder and 30:1 L/D barrier screw, a start-up barrel profile for Bapolene 152A is commonly set to 150/160/170/180°C from feed to metering zones, with adapters and die maintained at 180–190°C. The profile is adjusted to hold melt temperature at the die entrance in the 175–195°C range. A screen pack of 20/40/60 mesh is usually sufficient for film-grade LDPE because gel counts are low, but reworked material may require finer filtration. The recommended die gap is 0.8–1.2 mm, and the frost line is normally held at 8–10 die diameters. Blow-up ratios of 2.0:1 to 3.5:1 provide stable bubbles; operation above 4.0:1 is possible only with well-centered air rings and limited ambient drafts. Cast-film conversion is not the primary intended route for this grade, although it can be cast if melt temperature is reduced to 165–175°C to limit neck-in. Published data for this specific configuration is limited.
Long-chain branching is the dominant structural variable controlling Bapolene 152A’s blown-film response. Under extensional flow, branched chains create strain hardening that stabilizes the bubble and reduces draw resonance. That behavior permits the film to be drawn to thicknesses near 25 µm on conventional LDPE lines without the heavy melt fracture seen in narrow-distribution LLDPE. The same branching increases low-shear viscosity, so melt pressure at a given output remains higher than for HDPE of the same melt index. In distributive mixing sections, the broad molecular weight distribution lowers the threshold for wall slip and may reduce the intensity of melt-temperature overshoot. However, the stabilization is not unlimited: at frost line heights below 4 die diameters with high air-ring velocity, the bubble surface may oscillate because the polymer is quenched before sufficient chain relaxation occurs. Converters should record bubble diameter variation at the frost line every 30 min during start-up; a diameter variance greater than ±5% indicates that the air ring, die centering, or melt temperature requires correction. The resin’s long-chain branching also broadens the sealing window compared with high-density polyethylene, but seal initiation temperature remains higher than that of ethylene-vinyl acetate copolymers.
No predrying is required for Bapolene 152A when pellets are transferred directly from a dry warehouse. If the resin is stored in an unheated bay and moved into a warm production room at relative humidity above 60%, surface condensation may occur; in that condition, the pellets should be brought to 20–25°C and the conveying air should be dried before extrusion. The maximum recommended melt temperature is 220°C; sustained operation above this value can generate oxidized gel particles and may shift adhesion of the film into the collapsing frames. The grade should not be blended with polypropylene or high-density polyethylene at high addition levels without evaluating density shift, seal initiation, and optical degradation. Recycled film regrind can be incorporated, but no published data for this specific configuration is available for additions above 30%. If high concentrations of calcium carbonate masterbatch are added, dart impact and tear resistance fall at a rate that is strongly dependent on filler particle size and coating; the converter should verify those properties on the specific film line rather than extrapolating from small-scale laboratory tests.
Seal initiation in LDPE film is determined by the temperature at which the fusion bond reaches a specified peel strength. For a 50 µm film, Bapolene 152A typically requires a sealing jaw temperature between 105°C and 120°C at a dwell time of 0.5 s; hot-tack strength at 110°C is commonly sufficient for collation shrink overwrap. These values should be measured by ASTM F2029 or ASTM F88 on the finished film, because sealant performance shifts with gauge, contamination, and additive package. The broad melting range of low-density polyethylene gives a flat sealing curve, but it also means that high sealing temperatures can cause burn-through at thin-gauge sections. Converters should therefore monitor seal-bar temperature with infrared pyrometry at startup and after gauge changes.
Downgauging a 1.5 g/10 min LDPE film below 30 µm does not reduce tensile strength proportionally, but it changes the hierarchy of failure modes. Above 50 µm, dart impact and tear propagation dominate; below 25 µm, pinhole formation, blocking, and gauge variation become the controlling defects. Bapolene 152A can be drawn to 20 µm on high-speed lines if the die gap is kept at 0.8–1.0 mm and the frost line is lowered to 6–8 die diameters. However, optical properties measured on 50 µm film do not transfer to 25 µm film because surface roughness and internal haze scale with quench rate and draw. The dart drop value at 25 µm is typically less than half the value at 50 µm, and the Elmendorf tear in the machine direction can become limiting. Converters should audit seal strength and hot-tack every 2 h when running downgauged collation shrink film because gauge deviations at the layflat are amplified by the shrink ratio.
Typical film structures using Bapolene 152A include 75–125 µm industrial liners, 40–60 µm heavy-duty sacks, 25–50 µm collation shrink overwrap, and 30–80 µm agricultural sheeting. The choice of this grade over other LDPE film grades is normally driven by melt flow and density equivalence, not by additive concentration. In distributor comparisons, the grade is positioned as a general-purpose LDPE with optical quality suitable for clear overwrap but without the high-slip and antiblock levels required for high-speed form-fill-seal operations; those properties are achieved by adding a slip/antiblock masterbatch at 2–5% by weight, depending on equipment configuration. Regulatory compliance for food-contact applications is commonly evaluated under FDA 21 CFR 177.1520 for olefin polymers. Bapolene 152A may be considered for food contact if the finished article meets the extractable limits and end-use restrictions in the applicable paragraph. European food-contact compliance, if claimed, must be confirmed against EU Regulation 10/2011 and the specific migration limits for monomers and additives. The product is not a medical-grade resin unless a separate regulatory letter is issued by the seller. Customers seeking REACH or RoHS declarations must obtain the current safety data sheet and product compliance statement for the production lot; general statements in commercial brochures are not sufficient for record-keeping.