| HS Code | 257323 |
| Productname | tert-Butyl Peroxy-2-Ethylhexanoate (TBPEH) |
| Chemicalname | tert-Butyl peroxy-2-ethylhexanoate |
| Synonyms | tert-Butyl 2-ethylhexaneperoxoate; TBPEH; 2-Ethylhexaneperoxoic acid tert-butyl ester |
| Casnumber | 3006-82-4 |
| Ecnumber | 221-110-7 |
| Molecularformula | C12H24O3 |
| Molecularweight | 216.32 g/mol |
| Activeoxygencontent | 7.4% |
| Appearance | Clear liquid |
| Physicalstate | Liquid |
| Color | Colorless to pale yellow |
| Odor | Mild ester-like |
| Density | 0.92 g/cm3 at 20°C |
| Boilingpoint | 248°C |
| Flashpoint | 77°C |
| Refractiveindex | 1.438 at 20°C |
| Viscosity | 5.5 mPa.s at 20°C |
| Solubilityinwater | Insoluble |
| Solubilityinorganicsolvents | Soluble |
| Tenhourhalflifetemperature | 72°C |
| Assay | >=98% |
As an accredited tert-Butyl Peroxy-2-Ethylhexanoate (TBPEH) factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.
| Packing | TBPEH is supplied in 25 kg UN-approved polyethylene drums, sealed, labeled as organic peroxide, and stored cool. |
| Container Loading (20′ FCL) | 20′ FCL loading of tert-Butyl Peroxy-2-Ethylhexanoate (TBPEH): hazardous organic peroxide, palletized drums, properly secured, temperature-controlled, ventilated, DG-labeled, IMDG-compliant, and documented. |
| Shipping | TBPEH ships as UN 3106, Organic Peroxide Type D, liquid, temperature controlled, Class 5.2. Proper shipping name includes tert-Butyl Peroxy-2-Ethylhexanoate. Use approved peroxide packaging and comply with ADR/IMDG/IATA. Maintain control temperature at 20°C (emergency 25°C). Quantity limits and segregation rules apply; avoid heat, sunlight, and incompatible materials. |
| Storage | Store TBPEH in a cool, dry, well-ventilated, fire-resistant area away from heat, sparks, sunlight, and ignition sources. Keep in original, labeled, compatible containers. Maintain recommended temperature control. Segregate from acids, bases, reducing agents, accelerators, metals, and combustibles. Use explosion-proof equipment, secondary containment, and spill/emergency provisions. Prevent friction, impact, and contamination. Store only quantities needed. Consult SDS and local regulations. |
| Shelf Life | TBPEH shelf life is temperature-dependent: about 12 months at 10°C, 6 months at 20°C, and 3 months at 30°C. |
tert-Butyl peroxy-2-ethylhexanoate (TBPEH) operates as a medium-temperature peroxyester initiator with a representative 10 h half-life at 72 °C and 1 h half-life at 92 °C in chlorobenzene solution. The undiluted peroxide has an active oxygen content near 7.4 %, but commercial formulations are commonly supplied as 50 % solutions in odorless mineral spirits, plasticizer, or ester solvent to reduce friction sensitivity and permit mass-flow metering. TBPEH is employed in bulk and solution polymerization of styrenic and methacrylic monomers, in acrylic polyol resin synthesis, and in the thermal curing of unsaturated polyester and vinyl ester matrices, where its decomposition fragments remain compatible with non-polar and moderately polar polymer backbones. It is not recommended for polyolefin crosslinking or for high-temperature melt processing above about 160 °C, because the peroxide half-life is too short to provide uniform radical distribution and the resulting volatile decomposition products can create voids. The processing envelope overlaps with lower-temperature diacyl peroxides but extends into regions where dibenzoyl peroxide produces excessive aromatic residues.
In continuous mass polymerization of general-purpose polystyrene and high-impact polystyrene, TBPEH is metered as a 50 % solution into a stirred pre-polymerizer that is held at 115 °C to 125 °C. The pre-polymerizer is an anchor-agitated continuous stirred-tank reactor with an external recycle cooler; the agitator is typically a helical ribbon impeller sized for a mixture viscosity between 1,000 mPa·s and 10,000 mPa·s. Styrene conversion at the pre-polymerizer outlet is controlled to 15–30 wt% by adjusting the initiator feed and the jacket temperature, because the downstream gear pump and transfer line are specified for a limited pressure drop. TBPEH provides a useful radical flux under these conditions because its 1-h half-life at 92 °C is short enough to avoid large residual peroxide carryover into the finishing zone, yet long enough to maintain initiation during the average liquid residence time of 2–4 h. A production-scale limitation is the temperature gradient between the jacket and the stagnant film on the vessel wall; if the wall film exceeds 130 °C, local TBPEH consumption rises sharply and the bulk viscosity fails to follow the expected conversion curve. The resulting viscosity plateau can be 10–20 % lower than the reference batch, which reduces melt pump suction pressure and forces a lowering of the devolatilizer screw speed. Devolatilization is performed in a counter-rotating twin-screw extruder with an L/D ratio of 36:1 and a vacuum port below 20 mbar, reducing residual styrene below 0.1 wt% before melt filtration through a 40 µm screen. Melt flow rate is tested according to ISO 1133-1 and tensile properties are measured under ASTM D638. Batch-to-batch variation in the mineral oil carrier viscosity also affects the initiator pump calibration, which must be rechecked whenever the peroxide feed tank is replenished.
A glass-lined reactor operating at 110 °C receives TBPEH as a 50 % solution in mineral spirits to initiate high-solids acrylic polyol synthesis for two-component polyurethane clearcoats and pigmented basecoat resins. The monomer feed, containing n-butyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, 2-hydroxyethyl methacrylate, and styrene, is added over 4–6 h through a high-shear feed nozzle while TBPEH is co-fed to maintain a constant radical concentration. The reactor operates at 125–135 °C with reflux cooling, and the condenser duty is set by the solvent reflux rate. The limiting factor is not the peroxide half-life but the distribution of the oxidant and the hydroxy monomer across the liquid surface. Poor feed distribution creates methacrylate-rich microdomains that crosslink or gel, raising solution haze and increasing the pressure drop across the 5 µm bag filter. Molecular weight is monitored by gel permeation chromatography against polystyrene standards; the target weight-average molecular weight is 4,000 g mol−1 to 8,000 g mol−1 with a polydispersity index below 2.0. The final resin is adjusted to 1,000 mPa·s to 3,000 mPa·s at 23 °C under ISO 2555, hydroxyl value is determined by DIN 53240-2, and acid value is measured using DIN EN ISO 2114. Residual monomer is controlled below 0.3 wt% because unconverted acrylate raises the VOC content measured by ASTM D2369 and increases odor in the final two-component film. The acrylic polyol is crosslinked with an aliphatic polyisocyanate in a spray-applied clearcoat and is tested for cure and adhesion under ASTM D3359. If peroxide feed stops while monomer feed continues, the radical population decays and unreacted acrylate accumulates; restarting the initiator feed without reducing the monomer rate produces a mild autoacceleration event that can raise the batch temperature by 5–8 °C and shift the molecular weight below specification.
When continuous glass roving is pulled through a heated die, the unsaturated polyester resin bath is held at 20–30 °C and the die is divided into three temperature zones. TBPEH is introduced into the resin as a 50 % plasticizer-diluted peroxide or as a filler-dispersed paste, because unmixed peroxide can settle in a poorly agitated bath. The first die zone is held at 80–90 °C, the second at 100–110 °C, and the third at 120–130 °C, with pull speeds between 0.2 m min−1 and 0.6 m min−1 depending on profile thickness. The 1-h half-life at 92 °C positions TBPEH as an early die-inlet initiator: the resin begins to gel shortly after the roving enters the heated zone, and the peak exotherm is concentrated near the interface between the first and second zones. If the line speed is increased without raising the first-zone temperature, the profile exits the die with exposed glass, surface fiber breakout, and a Barcol hardness below 35 under ASTM D2583. If the first-zone temperature is raised above 95 °C to compensate, the gel time shortens and the pulling force rises to a level that can snap roving or seize the die. On a production line with a 600 mm heated die, the practical operating window between undercure and die blockage is frequently narrower than 10 °C. To widen this window, TBPEH is combined with tert-butyl peroxybenzoate in a binary initiator system: TBPEH supplies the initial radical flux at the die inlet, while tert-butyl peroxybenzoate survives into the final zone to complete cure and reduce residual styrene. This is necessary for structural profiles tested under ISO 527-4 for tensile behavior and ISO 14125 for flexural behavior. Glass content is verified by ASTM D2584, and dimensional tolerance is checked using ASTM D3917. Residual styrene in the finished profile is kept below 0.1 wt% because post-die emissions cause surface tack and regulatory non-compliance. The initiator loading must be recalculated when the roving supplier changes, because differences in sizing chemistry and moisture content shift the gel point by up to 15 s at the same die temperature.
Bisphenol-A epoxy vinyl ester laminates used for chemical storage tanks, scrubbers, and secondary containment liners are frequently post-cured with a staged temperature ramp that begins below 100 °C to avoid thermal stress between the corrosion barrier and the structural layer. TBPEH is selected in these systems when the fabricator requires an initiator that can be activated by mild external heat rather than one that depends entirely on room-temperature cobalt acceleration. In a hand lay-up or filament-wound structure, the vinyl ester resin is conditioned at 25 °C with a low-viscosity styrenated backbone and, where room-temperature gelation is required, a cobalt octoate promoter level of 0.1–0.5 phr based on resin. TBPEH is added separately at 0.5–1.0 phr; pre-mixing TBPEH directly with cobalt octoate before dispersion into the resin is avoided because the promoter accelerates decomposition into a rapid radical burst in the mixing bucket. The laminate gels at room temperature for 30–60 min and is then moved into a convection oven at 80 °C for 2–4 h, followed by 100 °C for 2 h. This staging reduces the residual styrene content to below 0.5 wt%, but only if the matrix glass transition temperature rises above the post-cure temperature. Chemical resistance is assessed under ASTM C581, and the laminate must show no blistering, no fiber blooming, and no weight change greater than ±5 % after immersion in the service medium. Thick sections above 12 mm are at risk of exotherm-driven stress cracking if the oven ramp begins too early. In fabrication practice for 1,000 L resin batches, laminates cured with TBPEH at 80 °C can develop internal cracks when the mid-laminate exotherm exceeds 120 °C before volatiles have escaped from the surface. For this reason, the ramp is delayed until the surface hardness measured by a Shore D durometer reaches 60.
In solution polymerization of methyl methacrylate with methacrylic acid, glycidyl methacrylate, or n-butyl methacrylate, TBPEH is injected into a jacketed reactor at 105–120 °C while the monomer mixture is fed over 3–5 h into an aromatic solvent or low-boiling ester blend. The peroxide is selected because its decomposition fragments are non-aromatic and do not contribute the benzoate odor associated with benzoyl peroxide, a property that matters when the copolymer is formulated into adhesives used in enclosed vehicle cabins. The free-radical flux is maintained by two separate initiator feed lines: the first delivers TBPEH with the monomer stream, and the second adds a small amount of a higher-temperature peroxide during the final 30 min to reduce residual monomer. The resulting copolymer is cooled and filtered; weight-average molecular weight is controlled between 20,000 g mol−1 and 80,000 g mol−1. Higher molecular weight leads to cohesive failure in the bonded joint, while lower molecular weight produces a polymer with insufficient film strength under ISO 4587 lap shear testing. The copolymer solution is analyzed by gas chromatography for residual methyl methacrylate, with the specification set below 0.1 wt%, because unreacted monomer in the final adhesive mixture shifts the activation energy for cure and generates volatile outgassing in the bond line. T-peel adhesion on treated aluminum is evaluated according to ISO 11339 after the copolymer is compounded with tougheners and a separate curing agent. Batches that exceed 130 °C during polymerization show a lower epoxide equivalent weight when glycidyl methacrylate is present, which alters the crosslink stoichiometry of the final adhesive and must be corrected by adjusting the hardener addition. Molecular weight distribution is also sensitive to the mineral oil carrier introduced with the TBPEH solution; this carrier remains in the copolymer and, above 0.5 wt%, can reduce the glass transition temperature measured by ISO 11357-2.
Once the methyl methacrylate syrup reaches a partially polymerized state, cast poly(methyl methacrylate) sheet production proceeds through a controlled thermal ramp. TBPEH is dissolved into the monomer at 0.05–0.2 wt% before the batch is heated in a water bath at 70–80 °C. The 10-h half-life at 72 °C produces a steady radical concentration during the slow thickening stage, allowing the syrup to reach 15–25 % conversion before it is poured into a glass cell. Open cell filling at too high a syrup viscosity traps air bubbles; holding the syrup at 20 °C for 24 h after pre-polymerization allows dissolved gases to escape. The cell is then moved into a forced-air oven with a ramp from 60 °C to 110 °C over 6–10 h. The critical process variable is the heat of polymerization of methyl methacrylate, reported at approximately 57.7 kJ mol−1, because the insulating glass cell can develop a centerline temperature that is 20–30 °C higher than the oven set point if the initiator loading is too high. In cast sheet thicknesses above 15 mm, this exotherm produces visible bubbles and internal strain, reducing optical transmission below the level specified in ISO 13468-1. TBPEH is preferred over benzoyl peroxide for thick sheet because the peroxyester decomposition rate is less sensitive to remaining monomer concentration and the resulting sheet shows lower haze after post-cure at 120 °C for 2 h. Physical testing follows ASTM D4802 for acrylic sheet, including tensile strength and elongation measurements. Residual monomer in the finished sheet is controlled below 0.5 wt% to meet heat deflection performance under ISO 75-2. If the syrup conversion overshoots to 30 % before cell filling, the filled cell shows flow marks and thickness variation, and the final sheet fails thickness tolerance specified in the downstream cutting plan.
Competitive tert-Butyl Peroxy-2-Ethylhexanoate (TBPEH) prices that fit your budget—flexible terms and customized quotes for every order.
For samples, pricing, or more information, please contact us at +8618963613625 or mail to sales10@ascent-petrochem.com.
We will respond to you as soon as possible.
Tel: +8618963613625
Email: sales10@ascent-petrochem.com
Flexible payment, competitive price, premium service - Inquire now!
tert-Butyl peroxy-2-ethylhexanoate (TBPEH) is supplied as a liquid peroxyester with the molecular formula C12H24O3, CAS 3006-82-4, and molecular weight 216.32 g/mol. Commercial grades are distributed under designations including Trigonox 21S and Luperox 26, with principal configurations comprising an undiluted 97% technical liquid, 50% solutions in dearomatized aliphatic hydrocarbon, and plasticized pastes. The undiluted grade is specified by an active-oxygen content near 7.18 wt% against a theoretical value of 7.40 wt%, density of approximately 0.89 g/cm³ at 20 °C, and a clear liquid appearance with water and inorganic impurity levels controlled to the supplier’s release limits. The product functions as a thermal free-radical initiator for acrylate, methacrylate, styrenic, and unsaturated polyester systems, and as a curing agent for peroxide-cure thermoset and elastomer processes in which the cure temperature exceeds the decomposition onset.
Thermal decomposition of TBPEH follows first-order kinetics in dilute solution; the apparent activation energy derived from the 10-hour, 1-hour, and 1-minute half-life temperatures is approximately 125 kJ/mol. That value is used to correct residence time in heated feed lines and to calculate adiabatic heat accumulation. Because the compound is a peroxyester rather than a dialkyl peroxide, decomposition is sensitive to solvent polarity and to the presence of dissolved metal ions. Half-life data are therefore not transferable from solvent to monomer without adjustment.
| Initiator | Physical form at 25 °C | 10-h half-life | 1-h half-life | 1-min half-life |
|---|---|---|---|---|
| TBPEH | Liquid | 73 °C | 92 °C | 133 °C |
| Dibenzoyl peroxide | Solid | 73 °C | 92 °C | 131 °C |
| tert-Butyl peroxybenzoate | Liquid | 104 °C | 124 °C | 166 °C |
| Azobisisobutyronitrile | Solid | 65 °C | 82 °C | 117 °C |
Release specifications for the undiluted liquid are defined by iodometric active-oxygen assay, density by ASTM D4052, and color by Pt-Co scale. The active-oxygen content is the primary purity indicator and is used to adjust metering rates in production. Viscosity at 20 °C is typically 2.0–4.0 mPa·s, which permits transfer with gear or diaphragm metering pumps through 6–10 mm stainless-steel lines at ambient temperatures below the control temperature. Refractive index at 20 °C is commonly controlled in the range 1.428–1.432; color for the technical liquid is generally below 30 Pt-Co units. Water content is held below 0.10 wt% because free water accelerates metal-contact decomposition and can cause localized pressure increases in closed storage.
Formulated grades are not interchangeable by volume. The 50% hydrocarbon solution contains approximately 3.6 wt% active oxygen and has a higher self-accelerating decomposition temperature than the neat ester because the solvent absorbs heat and dilutes the peroxide. The exact phlegmatizer composition must be checked for compatibility with the resin system; aliphatic hydrocarbon may influence cure rate and final surface gloss in open molding. Pastes are rarely used in automated liquid-handling lines but are specified where vertical surface retention is required.
In sheet molding compound and bulk molding compound operations, TBPEH is metered into unsaturated polyester resin at addition levels of 1.0–2.0 phr based on resin solids. Press temperatures between 120 °C and 150 °C are common because the half-life at 130 °C is short enough to initiate crosslinking through the part thickness while allowing resin flow before gelation. Compared with dibenzoyl peroxide paste, which requires a solid dispersion or plasticizer carrier, TBPEH does not add particulate matter to doctor boxes and minimizes benzoic acid bloom. Compared with tert-butyl peroxybenzoate, the lower half-life temperature permits cure at lower tool settings but narrows the storage and handling margin.
Control of cure is performed using exotherm curves from instrumented molds. The peak exotherm and time-to-peak are recorded with thermocouples placed at the part center; acceptance limits are set on production tooling because mold steel, heating-channel geometry, and filler thermal conductivity alter heat transfer. Barcol hardness after demolding is checked under ASTM D2583; residual styrene is measured by gas chromatography in many operations. Flexural properties are determined under ISO 178 or ASTM D790, and heat deflection temperature under ISO 75-2 or ASTM D648 as part of first-article qualification. Published data for specific SMC formulations containing TBPEH are available in resin supplier technical bulletins, but values are not transferable across filler types and glass loadings.
In bulk, suspension, and solution polymerization of styrene and acrylic esters, TBPEH is added at 0.05–0.50 wt% on monomer, depending on molecular weight target and reactor cooling capacity. The initiator is often used as the intermediate-temperature component in a staged initiator system: a lower-temperature azo initiator starts the reaction at 70–80 °C, TBPEH maintains radical flux through the viscosity rise, and a higher-temperature peroxide such as tert-butyl peroxybenzoate reduces residual monomer at the end. Because TBPEH is a liquid, mass polymerization plants meter it directly into continuous stirred-tank reactors or recycle loops through stainless-steel diaphragm pumps. The feed system is designed with relief valves and rupture discs because decomposition gas formation in a blocked line can cause pressure accumulation.
Thermal homolysis of TBPEH yields tert-butoxy and 2-ethylhexanoyloxy radicals; the acyloxy radical decarboxylates to carbon dioxide and a branched alkyl radical. Decomposition products therefore include tert-butanol, acetone, carbon dioxide, and 2-ethylhexanoic acid-related species. The aliphatic profile reduces aromatic bloom on molded surfaces compared with dibenzoyl peroxide and tert-butyl peroxybenzoate. Volatile byproducts require vacuum venting in closed tools; accumulation of acetone and tert-butanol at the tool surface can produce gloss variation and, in severe cases, voids. For large marine or sanitary panels, ventilation design is specified according to NFPA 91 or applicable mechanical code requirements, and the resin formulation is adjusted to control exotherm and surface air release.
Compared with azobisisobutyronitrile, TBPEH does not introduce nitrile decomposition fragments; however, it does produce carbon dioxide and volatile oxygenated species, so continuous mass polymerization lines must provide venting at the devolatilization stage. In suspension polymerization, the liquid peroxide partitions into the monomer phase, whereas water-soluble initiators such as hydrogen peroxide require pH-controlled aqueous-phase handling. TBPEH is not a room-temperature redox initiator and should not be compared directly with methyl ethyl ketone peroxide/cobalt systems.
In continuous lamination and pultrusion, TBPEH is injected at the mix head downstream of high-shear mixing. The liquid initiator is not added to the styrene monomer tank before mixing because localized decomposition can occur in solar-heated outdoor storage. Barrel or bath residence time is kept below one half-life at the processing temperature; for a pultrusion die set at 130 °C, the half-life is approximately 1–2 minutes, and line speed is adjusted so that the material exits the die only after peroxide consumption is substantially complete. Die temperatures above 140 °C are used to complete cure after gelation, but the exotherm in large profiles can generate internal cracking if line speed is increased without recalibrating zone temperatures.
The self-accelerating decomposition temperature of the neat 97% liquid is commonly reported as 35 °C. Under the UN model, the control temperature is 25 °C and the emergency temperature is 30 °C. Refrigerated storage at 15–25 °C is applied in insulated, ventilated rooms with defrosting designed to avoid local hot spots. The 50% hydrocarbon solution has a higher SADT and may be shipped without temperature control depending on package size and competent-authority classification; supplier documents govern. The neat product is assigned to Class 5.2 organic peroxide, with transport designation UN 3113 or UN 3115 for temperature-controlled type C or D liquid peroxide. Shippers must classify the exact package and concentration using UN Test H.4 data and the dangerous goods list.
Storage and handling follow NFPA 432 for organic peroxide formulations and 29 CFR 1910.1200 hazard communication. The product is kept away from accelerators, cobalt octoate, iron naphthenate, amines, strong acids, and strong reducing agents. Separate spill-control materials are used because cellulosic rags contaminated with organic peroxide can self-ignite after solvent evaporation. Firefighting is by water spray for cooling, not by carbon dioxide or dry chemical alone, because the peroxide supplies oxygen. Engineering controls include local exhaust ventilation at feed stations, explosion-proof electrical classification in areas where vapor can accumulate, and bonding and grounding of transfer lines.
| Parameter | Reference or code | Typical limit or designation |
|---|---|---|
| Storage temperature | Supplier SDS / UN model | 15–25 °C for 97% liquid |
| SADT | UN Manual of Tests and Criteria, Test H.4 | 35 °C for 97% liquid |
| Transport class | ADR / RID / IMDG Code | Class 5.2, UN 3113 or 3115 |
| Storage code | NFPA 432 | Organic peroxide storage separation |
| Assay method | Iodometric titration, internal release | 97% minimum for neat grade |
| Density method | ASTM D4052 | 0.89 g/cm³ at 20 °C |
Because the processing window of TBPEH is bounded by the control temperature on the cold side and the half-life on the hot side, transfer lines and recirculation loops are designed to eliminate dead zones where material can remain for extended time. In high-temperature continuous processes, the feed cabinet is refrigerated below 25 °C, while the injection point is cooled or segregated from hot surfaces. Before substitution for another peroxide, the complete formulation must be screened in an adiabatic calorimeter and then on the production line with thermocouple mapping. The use of TBPEH in a given reactor or mold is therefore governed by SADT, half-life, solvent compatibility, venting capacity, and the specific equipment heat-transfer coefficient.