Cyclohexanone Peroxide Chp

Cyclohexanone Peroxide (CHP)

    VTB
    Specifications
    HS Code 466303
    Product Name Cyclohexanone Peroxide (CHP)
    Chemical Family Organic peroxide
    Iupac Name 1-Hydroperoxycyclohexyl 1-hydroxycyclohexyl peroxide
    Cas Registry Number 78-18-2
    Chemical Formula C12H22O5
    Molar Mass 246.30 g/mol
    Appearance White to off-white crystalline powder or paste
    Odor Mild characteristic odor
    Physical State At 20 C Solid or paste, depending on formulation
    Density 1.14 g/cm3 at 20 °C
    Melting Point 77-80 °C (decomposes)
    Decomposition Temperature 77-80 °C
    Solubility In Water Insoluble
    Solubility In Organic Solvents Soluble in acetone, benzene, chloroform, and other organic solvents
    Oxidizing Properties Strong oxidizing agent
    Vapor Pressure Very low; negligible at ambient temperature
    Hazard Class 5.2 Organic peroxide
    Un Number 3104 (solid type C); 2119 for certain paste or mixture formulations
    Storage Temperature Below 25 °C, preferably refrigerated; away from heat, sparks, and sunlight
    Stability Heat-, shock-, and friction-sensitive; may decompose explosively
    Reactivity Reacts with acids, bases, reducing agents, and heavy metals
    Flammability Combustible; may ignite readily

    As an accredited Cyclohexanone Peroxide (CHP) factory, we enforce strict quality protocols—every batch undergoes rigorous testing to ensure consistent efficacy and safety standards.

    Packing & Storage
    Packing Cyclohexanone peroxide (CHP), 20 kg, desensitized, packed in UN-approved vented steel drum with polyethylene liner and oxidizer labels.
    Container Loading (20′ FCL) Load Class 5.2 CHP in a clean, dry 20′ FCL with DG placards, secure stowage, ventilation, segregation, and IMDG-compliant handling.
    Shipping Cyclohexanone peroxide (CHP) is typically shipped as UN 2119, Proper Shipping Name: Cyclohexanone peroxide, not more than 91% with water, Class 5.2 (Organic Peroxide), PG II. Use approved packaging, labels, placards, and documents; keep cool, away from heat, sparks, and incompatible materials; comply with IMDG/IATA/ADR/49 CFR.
    Storage Store cyclohexanone peroxide in small, clearly labeled, compatible containers, preferably wetted or phlegmatized as supplied. Keep in a cool, dry, dark, well-ventilated, fire-resistant area away from heat, sparks, flames, acids, reducing agents, metals, and combustibles. Prevent friction, shock, and impact. Limit access and quantities; follow local explosive-storage regulations. Use explosion-proof equipment and grounding/bonding where required. Never store near incompatible materials.
    Shelf Life Cyclohexanone peroxide has limited shelf life; it degrades with heat, light, and contaminants. Store cold and dark; monitor; never stockpile.
    Application of Cyclohexanone Peroxide (CHP)

    In open-mold unsaturated polyester resin (UPR) lamination, cyclohexanone peroxide (CHP) is metered into a resin pre-accelerated with cobalt octoate. The working dosage is 1.0–2.0 phr CHP with 0.2–0.5 phr cobalt octoate 6% metal content on resin mass. The redox pair decomposes to alkoxy radicals, initiating styrene–unsaturated polyester copolymerization at 25–30°C. Gel time under ASTM D2471 is held between 15 and 35 min for hand lay-up and spray-up. Peak exotherm is limited to 160°C in laminates thicker than 4 mm by reducing CHP to the lower end of the range and by allowing interpass cooling to 40–45°C. Direct mixing of undiluted CHP with cobalt accelerator is not permitted because neat contact can cause rapid decomposition. A wall-mounted catalyst doser or gun-mounted metering system injects CHP at 0.5–2.0% of resin flow, while a chopper gun deposits glass and catalyzed resin simultaneously in spray-up lines.

    The glass reinforcement schedule uses 300–600 g/m² E-glass chopped strand mat or woven roving. Laminating rollers consolidate the laminate and remove trapped air before gelation. Fiber content after cure is checked by ASTM D2584 and typically falls in the 30–40 wt% range. Styrene emissions from open-mold operations in the United States are subject to 40 CFR Part 63 Subpart WWWW; the lower exotherm of CHP relative to methyl ethyl ketone peroxide (MEKP) reduces monomer boil-off at the laminate surface. Cured laminates are qualified to ISO 527-2 for tensile strength, ISO 178 for flexural strength, and ASTM D256 for Izod impact. Typical tensile strength is 60–80 MPa, flexural strength is 100–150 MPa, and Barcol hardness after 24 h is 35–45. Terminal parts include boat hulls, chemical storage tanks, cooling tower shells, truck body panels, and sanitary ware.

    Indicative effect of CHP dosage on pot life and peak exotherm for an orthophthalic UPR with 0.4 phr cobalt octoate (6% Co) at 25°C, ASTM D2471 method.

    CHP dosage (phr)Gel time at 25°C (min)Peak exotherm (°C)
    0.550–7060–80
    1.028–4090–110
    1.516–24120–140
    2.08–14145–165
    2.54–8160–180
    3.02–5175–195

    Why Does Cobalt-to-CHP Ratio Dictate Through-Cure in Castings?

    Unfilled and lightly filled UPR castings are sensitive to the cobalt-to-CHP ratio because both under-acceleration and over-acceleration produce subsurface defects. A standard casting formulation uses 1.0–2.0 phr CHP and 0.2–0.4 phr cobalt octoate 6% metal. At 25°C, gel time is adjusted to 20–60 min for clear casting and 10–30 min for pigmented casting. If cobalt is below 0.15 phr, through-cure remains incomplete in sections above 10 mm; if CHP exceeds 2.5 phr, peak exotherm can exceed 170°C and internal cracking occurs. Clear embedment molds are therefore fitted with thermocouples and the exotherm is capped at 120–140°C. Residual styrene after cure is determined by gas chromatography under ISO 4901; post-cure at 60–70°C for 2–4 h lowers residual monomer and residual CHP decomposition byproducts.

    Certain pigments adsorb cobalt and change gel time. Carbon black and iron oxide are the most aggressive; compensation of 0.05–0.1 phr cobalt octoate is made only after gel-time verification under ASTM D2471. Molds with intricate undercuts are demolded at 50–70% of final hardness to reduce breakage; full hardness is reached after 24 h at ambient temperature. Castings are tested by ISO 527-2 for tensile strength, ISO 178 for flexural strength, and ISO 868 for Shore D hardness. Terminal products include buttons, decorative knobs, paperweights, transparent embedments, and display items. Compliance for decorative castings is handled through REACH (EC) No 1907/2006 and CLP Regulation (EC) No 1272/2008; food-contact castings require separate migration testing and are outside the standard CHP-cured resin specification unless explicitly demonstrated.

    Mineral-Filled Unsaturated Polyester Solid Surface Casting

    Solid surface matrices are compounded with 55–65 wt% alumina trihydrate (ATH) and, in some grades, 0–20 wt% silica or quartz filler. CHP is added at 0.8–1.5 phr and cobalt octoate at 0.2–0.4 phr. ATH releases water at temperatures above 180°C; peak exotherm is therefore limited to 140°C to preserve opacity, reduce porosity, and prevent crack formation in 10–25 mm slabs. Vacuum mixing at –0.09 to –0.095 MPa removes entrained air before catalyst addition. The catalyst is mixed last under low shear because high shear raises batch temperature and reduces pot life to 10–20 min. Vibration tables with 0.1–0.3 mm amplitude and 3,000–6,000 rpm consolidate the filled mix in closed molds. Demolding occurs at 60–90 min, followed by 24 h at 25°C and post-cure at 70–80°C for 2–3 h.

    Finished solid surface sheets are qualified under ANSI/ICPA SS-1-2018 or ISO 19712:2017. Tensile strength is tested by ISO 527-2, flexural strength by ISO 178, water absorption by ASTM D570, and surface hardness by ISO 868. A 12 mm cast sheet typically shows flexural strength of 45–60 MPa and tensile strength of 20–30 MPa. Flame-spread classification under ASTM E84 may be required for commercial interior installations. Terminal products are sinks, vanity tops, worktops, laboratory casework, and wall panels. Translucency is controlled by refractive index matching or mismatch between the ATH filler and the cured resin, so CHP-related exotherm and residual monomer variation directly affect color consistency between casts.

    At 0.6–0.8 mm wet film thickness, air-sprayed gelcoat formulated with CHP sets in 8–20 min at 25°C when the resin contains 0.3–0.5 phr cobalt octoate and 1.5–2.5 phr CHP. The spray mix is adjusted to 0.8–1.2 Pa·s under ISO 2884-1, with thixotropic index of 2.5–4.0 to prevent sag on vertical mold surfaces. Plural-component spray equipment or batch mixing is used; pot life after catalyst addition is 12–25 min. The gelcoat is deposited at 400–600 µm dry film thickness as a barrier layer before structural laminate is applied. Surface tack is eliminated by incorporating a small amount of paraffin or by using an air-curable resin, because atmospheric oxygen inhibits CHP/cobalt cure in the outer 10–20 µm. Cured film hardness is checked by ISO 868, adhesion by ISO 2409, and gloss retention after accelerated aging. Styrene emissions from gelcoat spraying are covered under 40 CFR Part 63 Subpart WWWW in the United States and Directive 2010/75/EU in the European Union. Terminal products include marine hull gelcoats, wind energy nacelle covers, shower trays, and exterior cladding panels.

    When Vinyl Ester Linings Are Post-Cured After Room-Temperature CHP Initiation

    Vinyl ester resins used for chemical-resistant linings are accelerated with cobalt and dimethylaniline (DMA) before CHP is added at 1.0–2.0 phr. The cobalt level is 0.3–0.5 phr and DMA is 0.05–0.1 phr. DMA secures surface cure but compresses pot life to 15–30 min at 25°C. Catalyzed resin is therefore applied by roller or airless spray within the first third of pot life. Lining thickness of 0.5–2.0 mm is built in multiple passes; each pass is allowed to reach 35–45°C internally before the next is applied. After 24 h ambient cure, the lining is post-cured at 70–80°C for 4 h to complete methacrylic conversion and improve solvent resistance. Peak exotherm is limited to 150°C to avoid microcracking at the steel–laminate interface.

    Chemical resistance is qualified by ASTM C581 with 90-day exposure to representative acid, caustic, and solvent fluids. Hardness retention, flexural strength retention, and visual rating are recorded. Pull-off adhesion to blasted carbon steel is tested by ISO 4624; values of 5–7 MPa are expected where surface preparation meets Sa 2.5. Terminal products include tank linings, sumps, scrubbers, and secondary containment areas. In such service, CHP-initiated room-temperature cure is selected when post-cure heat is available but on-site pot life and moderate exotherm are required. Storage of the peroxide must remain below 30°C and away from cobalt and DMA concentrates to avoid pre-reaction.

    Exotherm Management Determines Repairability of Polymer Concrete Overlays

    Polymer concrete repair mortars use an unsaturated polyester or vinyl ester binder with 10–13 wt% polymer content and graded silica or basalt aggregate. CHP is added at 1.0–2.0 phr based on resin weight, with cobalt octoate at 0.3–0.5 phr and DMA at 0.05–0.1 phr for low-temperature repairs at 5–15°C. Aggregate moisture is held below 0.1% because water consumes cobalt and retards cure. A forced-action mixer blends the resin component with aggregate for 2–3 min before catalyst injection; placement is completed within 10–15 min after catalyst addition. Overlays are screeded and troweled at 5–25 mm thickness. The lower exotherm of CHP relative to MEKP becomes critical in sections above 15 mm; peak exotherm is held under 90°C to prevent thermal shrinkage cracks and debonding from concrete. Compressive strength after 24 h is tested by ASTM C579, with typical values of 80–110 MPa; flexural strength is tested by ASTM C580 and often exceeds 20 MPa. Terminal products include chemical-plant drains, trench drains, bridge overlay repairs, and secondary containment floors.

    For closed-mold perfusion and resin transfer molding (RTM) operations, CHP is selected when low exotherm is required for thick cores or dimensionally stable tools. The resin is formulated at 0.15–0.30 Pa·s at 25°C for infusion; CHP dosage is 0.8–1.5 phr with cobalt octoate 0.2–0.4 phr. Injection time is kept below 50% of pot life to avoid viscosity rise in feed lines; pot life at 25°C is 25–45 min. Tooling is held at 30–45°C to stabilize gel time and through-cure. The low exotherm allows infusion of 20–40 mm core structures without exceeding 140°C in the laminate. After fill, the part remains under –0.07 to –0.09 MPa vacuum until gelation to prevent air ingress. Cured fiber volume fraction is measured by ASTM D3171 or ISO 1172 and is typically 50–60 vol% for carbon fiber RTM. Mechanical properties are qualified by ISO 527-2, ISO 178, and ISO 14130. Terminal products include wind turbine root sections, marine structural members, composite doors, and pump housings.

    Free Quote

    Competitive Cyclohexanone Peroxide (CHP) prices that fit your budget—flexible terms and customized quotes for every order.

    For samples, pricing, or more information, please contact us at +8618963613625 or mail to sales10@ascent-petrochem.com.

    We will respond to you as soon as possible.

    Tel: +8618963613625

    Email: sales10@ascent-petrochem.com

    Inquiry

    Get Free Quote of Ascent Petrochem Holdings Co., Limited

    Flexible payment, competitive price, premium service - Inquire now!

    Certification & Compliance
    More Introduction

    Cyclohexanone peroxide (CHP) is an organic peroxide supplied primarily as a 50% paste in phthalate plasticizer or as an aqueous emulsion, with commercial designations including CHP-50 and CHP-50E. The active oxygen content of a typical CHP-50 paste falls between 4.0% and 4.5%, while Brookfield viscosity at 25 °C is normally reported in the range 20 000–50 000 mPa·s. Density for the paste form is typically 1.05–1.15 g/cm³. CHP functions as a room-temperature radical initiator for unsaturated polyester and vinyl ester resins when used with cobalt carboxylate accelerators. The decomposition pathway is cobalt-mediated at ambient temperature, which distinguishes the product from benzoyl peroxide systems that require amine promotion or external heat. Under CLP Regulation (EC) No 1272/2008, formulated pastes may carry hazard statements H242, H315, H319, H335, and H410, depending on concentration. Storage is specified at or below 30 °C in vented containers, and the self-accelerating decomposition temperature (SADT) of commercial paste forms is generally above 50 °C. Gel time is not a fixed product property; it is determined according to ISO 2535 and varies with resin unsaturation, accelerator metal content, peroxide dosage, and temperature.

    ParameterCHP-50 pasteCHP-50E emulsionTest method
    AppearanceWhite to off-white pasteMilky white emulsionVisual
    Active oxygen4.0–4.5%4.0–4.3%ASTM E298
    Viscosity, 25 °C20 000–50 000 mPa·s500–2 000 mPa·sISO 2555
    Density, 25 °C1.05–1.15 g/cm³1.00–1.10 g/cm³ISO 2811-1
    SADT≥50 °C≥50 °CUN Manual of Tests and Criteria, Part II
    Storage temperature≤30 °C≤30 °CSupplier safety data sheet

    Processing use spans ambient-cure laminating, gelcoat, casting, polymer concrete, solid surface, and chemical anchor formulations. In unsaturated polyester resins, CHP-50 paste is metered at 0.5–2.0 phr, with cobalt octoate 6% metal added at 0.2–0.5 phr. At 20 °C, gel times between 10 min and 60 min are common, but the value is resin-specific. In vacuum infusion and resin transfer molding, CHP-50E emulsion may be selected because lower viscosity permits more uniform injection and reduces metering pump wear. Chemical anchor cartridges require temperature conditioning to 20–25 °C before use; low-temperature extrusion increases static mixer pressure and can produce streaking in the mixed adhesive.

    What Differentiates CHP from Methyl Ethyl Ketone Peroxide in Ambient-Cure Unsaturated Polyester Systems?

    Methyl ethyl ketone peroxide (MEKP) is the more common ambient-cure initiator, but CHP differs in cure profile rather than in chemical class alone. Both are ketone peroxides and both are promoted by cobalt salts, yet CHP produces a lower peak exotherm and a longer gel-to-cure interval in most unsaturated polyester systems. The lower exotherm reduces thermal stress in thick castings and can permit larger single pours without cracking. MEKP, by comparison, typically exhibits higher active oxygen content, often above 9% in commercial MEKP-50 grades, and faster gel development at equivalent cobalt loadings. The practical consequence is that CHP is not a drop-in replacement for MEKP where rapid demold is the controlling parameter. Reformulation is required because the accelerator/peroxide ratio must be rebalanced to maintain the same gel time. Comparative exotherm measurements made in accordance with the general method of ISO 2535 show formulation-dependent differences; published data for direct substitution in all resin classes is limited. The shift in gel-to-cure interval also affects secondary bonding and residual styrene levels, so post-cure time should be extended or post-cure temperature raised when CHP replaces MEKP.

    Batch-to-batch cobalt variation in formulated resin can shift gel time by 10–20% at fixed peroxide loading. Production-scale gelcoat operations therefore control cobalt by inductively coupled plasma analysis before peroxide addition. The peroxide paste itself contributes minor viscosity variation, but active oxygen drift outside ±0.2% of the supplier target may require dosage adjustment. Ambient moisture above 60% RH can retard surface cure in open molds; paraffinic surfacing agents or forced air ventilation are used instead of increasing peroxide because higher peroxide raises exotherm rather than surface conversion. These process boundaries are rarely visible in resin technical data sheets and are established by production-scale trials.

    Polymer concrete and solid surface castings exploit the lower exotherm of CHP. In pours above 50 mm section thickness, thermal cracking is controlled by keeping peak exotherm below the cured resin heat deflection temperature. CHP-based systems are typically selected when MEKP exotherm produces surface cracks or internal voids. Published exotherm data for specific resin systems is limited; production trials with embedded thermocouples are used to map peak temperature against part thickness and mold thermal conductivity. Barcol hardness development measured by ASTM D2583 is slower than MEKP-based systems at 20 °C, but post-cure at 40–60 °C for 2–4 h closes the conversion gap in many castings. Chemical anchor formulations use CHP because the lower exotherm reduces thermal degradation of the surrounding concrete and improves consistency in large-volume holes. Static mixer equipment with 12–20 elements is common, and viscosity limits at 10 °C become a processing bottleneck; preconditioning to 20 °C is required rather than increasing accelerator dosage alone.

    Thermal Decomposition Thresholds and Storage Limits

    CHP is an organic peroxide and undergoes self-accelerating decomposition above its SADT. The SADT value is package-size dependent, and the value of 50 °C for paste grades applies to the smaller package configurations evaluated under the UN Manual of Tests and Criteria, Part II. Larger packaging and lower thermal conductivity shift the safe handling envelope. Storage areas are specified for vented containers at or below 30 °C; separation from cobalt accelerators, amines, strong acids, alkalis, and rust is mandatory because contamination can initiate decomposition at temperatures below the normal SADT. Do not return unused material to the original container. Decomposition generates heat and combustible gases; containers must not be sealed tightly. Firefighting guidance uses water fog for cooling and excludes dry chemical or carbon dioxide closing of containers. The hazard classification depends on formulation and package type; transport approval requires the SADT, package performance, and organic peroxide type to be assigned by the competent authority. No single UN number is assigned to all CHP formulations.

    When Thick Castings Replace Methyl Ethyl Ketone Peroxide Systems

    When a production process substitutes CHP for MEKP in cast sections above 50 mm, the processing window narrows because cure speed is depressed while exotherm is moderated. The mold temperature and ambient temperature must be controlled within ±5 °C to stabilize gel time. In open molds, heat transfer is lower than in steel molds; peak exotherm therefore occurs later and may be lower, but the total heat released remains the same. Cure progression should be monitored by Barcol hardness and residual styrene rather than gel time alone. ASTM D2583 values above 30 are typically required before demolding thick castings; if the value is lower, post-cure at 50 °C is specified. In marble and solid surface casting, CHP is combined with low-profile additives and alumina trihydrate fillers at loadings above 50 phr; the higher filler content reduces exotherm but also reduces wetting and increases mix viscosity. Production-scale experience shows that premature demolding of CHP-based castings causes edge rounding and secondary machining defects due to insufficient through-cure.

    Viscosity and Dispersion Behavior in High-Shear Mixing Equipment

    High-shear dispersion of CHP paste into filled resin systems requires attention to localized temperature rise. In dissolvers operating at tip speeds above 15 m/s, batch temperature can increase by 8–12 °C over 20–30 min depending on batch size and viscosity. A temperature interlock at 35 °C prevents approaching the lower storage stability limit. CHP-50E emulsion disperses more readily at low shear than paste, but water content can reduce the final cure in closed-mold applications unless post-cure is adjusted. The paste form is preferred for filled systems because the plasticizer carrier avoids water migration at the filler interface. Viscosity measurements by ISO 2555 are used to set drum and pipeline heating setpoints; at 15 °C, paste viscosity may double relative to 25 °C, causing metering pump cavitation. Metering pumps should be selected for suction lift below 1.5 m and line velocity above 0.3 m/s. Published data for a specific configuration is limited; process validation is required.

    Can Cyclohexanone Peroxide Replace Benzoyl Peroxide in Ambient Curing?

    Benzoyl peroxide (BPO) is a diacyl peroxide, not a ketone peroxide, and its ambient-cure mechanism is typically promoted by tertiary aromatic amines such as dimethyl-p-toluidine. CHP is promoted by cobalt carboxylates. Direct replacement is therefore not possible without changing the accelerator chemistry. BPO/amine systems are used in acrylic and some unsaturated polyester systems where cobalt soaps may cause unwanted color shift. CHP/cobalt systems tend to produce a different color response in clear castings; long-term color data is resin-specific. BPO pastes often require refrigerated storage below 40 °C depending on water content, while CHP pastes are generally stable below 30 °C. The difference in radical flux affects surface cure: BPO/amine systems can generate a harder tack-free surface in thin films, whereas CHP/cobalt may require paraffin or surfacing agent addition for air inhibition control. Selection between CHP and BPO is therefore driven by accelerator compatibility, color requirements, and exotherm constraints rather than peroxide cost alone.